short communications
Soft X-ray radiation-damage studies in PMMA using a cryo-STXM
aDepartment of Physics and Astronomy, SUNY Stony Brook, Stony Brook, NY 11794-3800, USA
*Correspondence e-mail: tobias.beetz@stonybrook.edu
Radiation damage sets a fundamental limit for studies with versus dose between 298 K and 113 K sample temperatures. At both temperatures the critical dose for bond breaking is ∼15 × 106 Gy.
cryo-methods are known to ease these limits. Here, measurements on mass loss and the decrease in the C=O bond density as measured by oxygen-edge XANES (NEXAFS) spectroscopy in thin films of poly(methylmethacrylate) (PMMA), studied in a vacuum, are reported. While cryo-methods allow more than 95% of the mass to remain at doses up to Gy, there is little difference in C=O bond densityKeywords: soft X-rays; radiation damage; PMMA; XANES; STXM.
1. Introduction
Radiation damage is a limiting factor in imaging at high resolution with 106 Gy are involved in 50 nm resolution imaging with soft X-rays (Sayre et al., 1977; Gölz, 1992). These doses are sufficient to cause immediate changes in living cells, and to produce noticeable mass loss and shrinkage in some specimens that are wet but chemically fixed (Williams et al., 1993). It is well known that cryo-methods can greatly reduce radiation damage in biological specimens (Glaeser & Taylor, 1978; Dubochet et al., 1987). Cryo-X-ray microscopy experiments at 113 K have shown essentially no observable mass loss at the 50 nm spatial resolution level with radiation doses up to ∼1010 Gy (Schneider, 1998; Maser et al., 2000). However, mass loss is not the only mechanism of radiation damage, and cryo-methods are found to improve but not eliminate degradation of high-resolution electron diffraction data (Glaeser & Taylor, 1978). Overall can be preserved while chemical bonds are not preserved. This suggests that cryo-methods may offer differing degrees of protection for spectroscopy, atomic-resolution imaging or diffraction than simple mass-loss measurements would suggest.
Basic considerations of image contrast indicate that doses of ∼Radiation-damage effects in soft et al. (1995) used carbon XANES to monitor the decrease in C=O bond density due to and the increase in C=C bond density due to crosslinking, in room-temperature PMMA films that were first baked at various temperatures. The C=O bond density was found to decrease exponentially with increasing dose, with a characteristic dose of ∼13 × 106 Gy. Coffey et al. (2002) studied several other thin polymer films with carbon XANES, and investigated the influence of atmospheric oxygen on the radiation-damage chemistry. These authors found that the damage rate in a helium atmosphere is slowed down by a factor of approximately 100 relative to air for their poly(ethylenetherephthalate) (PET) sample. Their experiments were also conducted at room temperature. These studies provide the background to our goal of examining radiation damage using XANES spectroscopy for samples at cryogenic and room temperatures.
have been studied by measuring the loss of X-ray absorption near-edge structure (XANES) spectroscopic resonances in thin organic films. Zhang2. Materials and methods
2.1. PMMA sample
A PMMA film prepared on top of a silicon nitride window served as our sample. The silicon nitride window was produced by back-etching silicon from a wafer with a nitride layer grown on it, resulting in 100 nm-thick silicon nitride windows. The PMMA (MW 950 KD PMMA C6 from MicroChem) was spun onto the window at 7000 r.p.m. from a solution 6% by weight in chlorobenzene. We note here that the high molecular weight of the PMMA used should not affect the relative molecular weight reduction since the G-factor is largely independent of the molecular weight (Dawes & Glover, 1996; Smith et al., 2001). The PMMA samples were baked at 423 ± 1 K for 2 h. The thickness of the PMMA layer was then measured using a Tencor Instruments Alpha-Step 200 profiler to be 580 ± 20 nm. The chemical structure of PMMA is shown in Fig. 1.
The carbonyl s(C=O) transition (Tinone et al., 1994). The decrease in intensity of this transition with increasing dose is used later to quantify the damaging effects.
gives rise to a peak in the oxygen XANES spectra at 531.5 eV (Fig. 3) which is due to the O 12.2. Experimental description
The data presented here were acquired using the Stony Brook cryo-scanning transmission X-ray microscope (cryo-STXM) (Maser et al., 2000), which is part of the X1A undulator beamline at the National Synchrotron Light Source (Winn et al., 2000). The imaging mode of the cryo-STXM was used to deliver a known dose to the specimen. This was achieved by scanning the specimen with a step size of 40 nm through the focal spot provided by a Fresnel zone plate with a diameter of 160 µm, a central stop diameter of 80 µm and 45 nm outermost zone width. A phosphor-coated with 6.6% at 525 eV (see §2.2.3) recorded the transmitted at each step. A typical focused during exposure was approximately 1.8 MHz, resulting in 1.1 MHz after transmission through the PMMA sample. The incident of 1.8 MHz corresponds to a of ∼7 photons s−1 nm−2 averaged over the central Airy disc of the zone-plate's point spread function. The exposure at liquid-nitrogen temperature was carried out using a 10 ms pixel dwell time whereas the room-temperature exposure was carried out using a 5 ms pixel dwell time. With the energy of the damaging X-rays tuned to 525.0 eV, the dose during such a scan was approximately 7.0 × 106 Gy at liquid-nitrogen temperature and approximately 3.7 × 106 Gy at room temperature (see §2.3 for details). After the dose scan, the spectroscopy mode of the cryo-STXM was used to record an oxygen XANES spectrum across the oxygen K-edge. Since radiation dose is defined as energy absorbed per mass, which in turn is proportional to the exposed area, the beam was defocused to ∼3.6 µm during spectrum scans to produce a dose of only ∼0.6 × 106 Gy per scan.1 The same absorbed energy was therefore put into a larger area, allowing for low-dose spectroscopy. The sequence of dose scan and spectroscopy scan was then repeated about 20 times to give a cumulative dose to the specimen of more than 108 Gy. Finally, an in-focus image with a lower dwell time and a larger step size over a larger field was taken to ensure that the specimen remained centred on the X-ray beam axis. Fig. 2 shows such images of dosed regions at both recording temperatures.
To normalize the recorded spectra, a spectrum of an area with no PMMA on the window was recorded at the beginning of each sequence and used as an I0 spectrum.
2.2.1. Sample conditions
The cryo-STXM with its vacuum chamber was designed to handle specimens cooled to liquid-nitrogen temperature. In the first set of experiments the PMMA sample was cooled down to liquid-nitrogen temperature prior to exposure. The sample was then allowed to warm up to room temperature, before Fig. 2(c) was acquired. The second experiment was conducted with the PMMA sample at room temperature.
2.2.2. Energy calibration
To calibrate the energy of the oxygen XANES spectra, we added O2 gas into the path of the X-ray beam. The strong absorption at 530.82 eV (Hitchcock, 1994) was then used to calibrate the spectra.
2.2.3. Detector calibration
Knowledge of the efficiency of the phosphor-coated photomultiplier detector is important for calculating the exact dose delivered to the sample. This was determined by comparing the count rate on the detector of a collimated beam of focused X-rays with the current measured on a photodiode that has an almost 100% efficiency (Funsten et al., 1997). The measured detector efficiency was about 6.6% at 525 eV.
2.3. Dose calculations
The skin dose (dose deposited in the e absorption length as
of an absorber) can be calculated using the 1/where E is the photon energy in eV, N is the number of photons per second absorbed by the sample, measured in kHz, is the efficiency of the detector, t is the exposure time in ms, is the density in g cm-3, A is the radiated area in µm2, d is the thickness and is the inverse absorption length in µm−1.
The 1/e absorption length can be expressed as
where re = 2.812 × 10−15 m, NA is Avogadro's number, A is the and f2 is the imaginary part of the complex which can be found from tabulated values (Henke et al., 1993). This gave, for example, an assumed absorption length for PMMA of = 1.1 µm at 525.0 eV. A typical dose during an exposure was approximately 7.0 × 106 Gy for an exposure at liquid-nitrogen temperature and approximately 3.7 × 106 Gy for an exposure at room temperature. During a spectral scan, a typical dose was ∼0.6 × 106 Gy. Note that the dose in a spectral scan is still a high dose even though we widened the X-ray beam to a diameter of ∼3.6 µm and used a short dwell time. The short dwell time is also the reason for the relatively low signal-to-noise ratio in the spectral scan.
2.4. Fitting the spectra
The absorption peak due to the C=O bond density was fitted with a Gaussian. The height of the Gaussian was later used to quantify the loss of the C=O bond density under radiation. We note here that although XANES spectra were recorded at doses exceeding 108 Gy we only used data up to ∼35 × 106 Gy for our analysis, since the fit of the C=O bond peak for higher doses could not be made with a high level of certainty.
To determine the mass loss, each spectrum was fitted with an average value at the low-energy (528.0–529.5 eV) and at the high-energy (538.5–540.0 eV) end of the spectrum (Fig. 3). The ratio of the two average values was used to determine the oxygen mass loss as a function of dose using differential absorption analysis (Engström, 1946).
3. Results and discussion
3.1. Spectroscopic observations
To quantify the loss of the carbonyl group, the heights of the C=O absorption peaks determined from the XANES spectra are plotted versus the dose in Fig. 4. The data were fitted according to
where a is the radiation dose, ac is called the critical dose for the loss of the C=O bond density and is the remaining C=O bond density after infinite radiation dose. The figure shows both curves for the PMMA sample at liquid-nitrogen and room temperatures. Table 1 summarizes the fitting coefficients obtained.
|
From the decay rate of the C=O bond density at both temperatures it can be concluded that the specimen temperature has no influence on preserving XANES signatures of the chemical state of the specimen, at least in this example system.
3.2. Mass loss
The dependence of mass loss on dose is shown in Fig. 4 for both temperatures. Following Coffey et al. (2002), the mass loss (or loss in optical density) can be quantified by
where b is the radiation dose, bc is called the critical dose and is the remaining after infinite radiation dose. The fitting coefficients are also summarized in Table 1. We note here that, for a confident value of at liquid-nitrogen temperature, more data at higher radiation doses would have to be collected. However, since the focus of this report is on spectroscopic limits, we did not investigate higher radiation doses.
Our critical dose of ∼18 × 106 Gy at 525.0 eV for the control experiment at room temperature is in good agreement with the previously obtained value of 13 × 106 Gy at 317 eV by Zhang et al. (1995) and 14 × 106 Gy at 315 eV by Coffey et al. (2002). The higher dose that we obtained in our measurements may be explained in part by the fact that an additional dose of ∼0.6 × 106 Gy was estimated to be applied while acquiring a spectral scan. As we have seen in §2.3, the dose during a spectral scan is relatively high even though the beam was defocused. A better quantitative measurement of the dose should therefore include more exact information on the dose delivered during such a spectral scan. We also note that the difference may be due to the fact that a different weighting of molecular dissociations is obtained at 525.0 eV than at 315 or 317 eV, respectively.
4. Conclusions
We have shown that the C=O bond in irradiated PMMA is broken at comparable rates at liquid-nitrogen and room temperatures. We have confirmed that cryogenic sample conditions are extremely effective for reducing mass loss, as is required for non-atomic-resolution imaging applications such as nanotomography (Wang et al., 2000; Weiss et al., 2000). However, cryogenic sample conditions do not have a measurable affect on the soft X-ray radiation dose sensitivity of chemical bonds, at least in this model case of XANES spectroscopy of PMMA with no water present. We note that PMMA is much more sensitive to radiation damage than many other polymers, and that there also may be significantly different mechanisms (such as free-radical formation) acting in the case of hydrated organic molecules. Further experiments to study radiation-damage effects on hydrated protein solutions are in preparation.
Footnotes
1During a spectrum scan the widened beam will drift slightly off the previously radiated area as we scan to higher energies. From alignment measurements we calculate that drift-off effects become important above 534 eV and reach a maximum at an energy of 540 eV, where 10% of the incident photons will be off the radiated area, corresponding to a systematic error of 0.1 in terms of the optical density.
Acknowledgements
We thank Jaan Mannik for the PMMA sample preparation, and Michael Feser, Sue Wirick and Barry Winn for great help with the cryo-STXM and for stimulating discussions. This research was carried out at the National Synchrotron Light Source, Brookhaven National Laboratory, and was supported by the NSF under grants ECS-0099893 and DBI-9986819.
References
Coffey, T., Urquhart, S. G. & Ade, H. (2002). J. Electron Spectrosc. Relat. Phenom. 122, 65–78. Web of Science CrossRef CAS Google Scholar
Dawes, K. & Glover, L. C. (1996). Physical Properties of Polymers Handbook, edited by J. E. Mark, ch. 41, pp. 557–576. New York: AIP Press. Google Scholar
Dubochet, J., Adrian, M., Chang, J. J., Lepault, J. & McDowall, A. W. (1987). Cryotechniques in Biological Electron Microscopy, edited by R. A. Steinbrecht & K. Zierold, pp. 114–131. Berlin: Springer-Verlag. Google Scholar
Engström, A. (1946). Acta Radiol. Suppl. 63, 1–106. Google Scholar
Funsten, H. O., Suszcynsky, D. M., Ritzau, S. M. & Korde, R. (1997). IEEE Trans. Nucl. Sci. 44, 2561–2565. Web of Science CrossRef CAS Google Scholar
Glaeser, R. M. & Taylor, K. A. (1978). J. Microsc. 112, 127–138. CrossRef CAS PubMed Web of Science Google Scholar
Gölz, P. (1992). X-ray Microscopy III, edited by A. G. Michette, G. R. Morrison & C. J. Buckley, Springer Series in Optical Sciences, Vol. 67, pp. 313–315. Berlin: Springer-Verlag. Google Scholar
Henke, B. L., Gullikson, E. M. & Davis, J. C. (1993). Atom. Data Nucl. Data Tables, 54, 181–342. CrossRef CAS Web of Science Google Scholar
Hitchcock, A. P. (1994). J. Electron Spectrosc. Relat. Phenom. 67, 1–132. CrossRef CAS Web of Science Google Scholar
Maser, J., Osanna, A., Wang, Y., Jacobsen, C., Kirz, J., Spector, S., Winn, B. & Tennant, D. (2000). J. Microsc. 197, 68–79. CrossRef PubMed CAS Google Scholar
Sayre, D., Kirz, J., Feder, R., Kim, D. M. & Spiller, E. (1977). Ultramicroscopy, 2, 337–341. CrossRef CAS PubMed Google Scholar
Schneider, G. (1998). Ultramicroscopy, 75, 85–104. Web of Science CrossRef CAS PubMed Google Scholar
Smith, A. P., Spontak, R. J. & Ade, H. (2001). Polym. Degrad. Stab. 72, 519–524. Web of Science CrossRef CAS Google Scholar
Tinone, M. C. K., Tanaka, K., Maruyama, J., Ueno, N., Imamura, M. & Matsubayashi, N. (1994). J. Chem. Phys. 100, 5988–5995. CrossRef CAS Web of Science Google Scholar
Wang, Y., Jacobsen, C., Maser, J. & Osanna, A. (2000). J. Microsc. 197, 80–93. CrossRef PubMed CAS Google Scholar
Weiss, D., Schneider, G., Niemann, B., Guttmann, P., Rudolph, D. & Schmahl, G. (2000). Ultramicroscopy, 84, 185–197. Web of Science CrossRef PubMed CAS Google Scholar
Williams, S., Zhang, X., Jacobsen, C., Kirz, J., Lindaas, S., van't Hof, J. & Lamm, S. S. (1993). J. Microsc. 170, 155–165. CrossRef Google Scholar
Winn, B., Ade, H., Buckley, C., Feser, M., Howells, M., Hulbert, S., Jacobsen, C., Kaznacheyev, K., Kirz, J., Osanna, A., Maser, J., McNulty, I., Miao, J., Oversluizen, T., Spector, S., Sullivan, B., Wang, S., Wirick, S. & Zhang, H. (2000). J. Synchrotron Rad. 7, 395–404. Web of Science CrossRef CAS IUCr Journals Google Scholar
Zhang, X., Jacobsen, C., Lindaas, S. & Williams, S. (1995). J. Vac. Sci. Technol. B13, 1477–1483. CrossRef Google Scholar
© International Union of Crystallography. Prior permission is not required to reproduce short quotations, tables and figures from this article, provided the original authors and source are cited. For more information, click here.