Study on two-dimensional small-angle X-ray scattering of in situ silica filled nanocomposite elastomer during deformation

CROSSMARK_Color_square_no_text.svg

aKyoto Institute of Technology, Graduate School of Science and Technology, Japan, and bKyoto Institute of Technology, Faculty of Engineering and Design, Japan
*Correspondence e-mail: yuko@kit.ac.jp

(Received 16 August 2006; accepted 13 March 2007; online 14 April 2007)

Morphological change of in situ generated silica particles was investigated by a time-resolved two-dimensional small-angle X-ray scattering technique and a simultaneous tensile measurement. The in situ silica particles with diameter ca 34 nm were homogeneously dispersed in a rubbery matrix and the morphological change of the particles was followed up to the elongation ratio α = 2 during stretching and from α = 2.5 during retracting. The observed two-dimensional small-angle X-ray scattering patterns agreed with the simulation results by Rharbi et al. [Europhys. Lett. (1999), 46, 472–478] where a shear displacement model was proposed for the deformation mode of their soft nanocomposite.

1. Introduction

Most of the particulate filler-filled rubber products are soft nanocomposites, although the concept of nanocomposites has been significantly expanded in this century. Reinforcement of rubber by inclusion of fillers such as carbon black and silica is very common in rubber technology (Kraus, 1965[Kraus, G. (1965). Reinforcement of Elastomers. New York: Interscience.]). Carbon black has been utilized in the rubber industry for about 100 years. The mechanism of reinforcement, however, is not yet fully understood. Not only the geometric factors such as size and shape and the content, but also the interfacial interaction between the particle and rubbery matrix must be taken into account in order to elucidate the reinforcement effect. One of the difficulties for the clarification of the role of nanofiller in the reinforcement is the aggregation of nanoparticles in the rubbery matrix, which was recognized in rubber products prepared by the conventional mechanical mixing technique. Therefore, a model nanocomposite with well dispersed nanoparticles in a rubbery matrix should be of much value for analyzing the reinforcement effect.

For the preparation of such a model, in situ silica filling is useful. The silica formation is based on the sol–gel reaction of tetraethoxysilane (TEOS) in a rubber matrix. The reaction of TEOS takes place in two steps, the hydrolysis and the condensation reactions, to produce SiO2. This sol–gel process has been originally noted for the preparation of inorganic glasses at lower temperatures (Brinker & Scherer, 1982[Brinker, C. J. & Scherer, G. W. (1982). Sol-Gel Science. New York: Academic Press.]). In the field of rubber science, crosslinked rubbers have been subjected to this in situ silica filling (Mark & Pan, 1982[Mark, J. E. & Pan, S.-J. (1982). Macromol. Chem. Rapid Commun. 3, 681-685.]; Mark, 1985[Mark, J. E. (1985). Science of Ceramic Chemical Processing, edited by L. L. Hench & R. D. Ulrich, ch. 47. New York: John Wiley & Sons.]; Kohjiya et al., 1994[Kohjiya, S., Yajima, A., Yoon, J. R. & Ikeda, Y. (1994). Nippon Gomu Kyokaishi, 67, 859-861.]; Kohjiya & Ikeda, 2000[Kohjiya, S. & Ikeda, Y. (2000). Rubber Chem. Technol. 73, 534-550.]). This method produces homogeneously dispersed nano-silica particles in the rubbery matrix.

In this paper, a morphological change of primary in situ silica particles in a rubbery matrix is reported by a simultaneous tensile and two-dimensional small-angle X-ray scattering (two-dimensional SAXS) measurement at the length scale of ca 10–220 nm.

Up to now, several studies on the deformation of soft nanocomposites have been reported. For examples, one of the pioneering works is a study on the deformation behavior of nanocomposites composed of Nanolatex and silica of ca 20 nm diameter by small-angle neutron scattering (SANS) under a slow elongation, where the obtained scattering patterns were compared with those by a computer simulation (Rharbi et al., 1999[Rharbi, Y., Cabane, B., Vacher, A., Joanicot, M. & Boue, F. (1999). Europhys. Lett. 46, 472-478.]). Together with several experimental studies (Rharbi et al., 1996[Rharbi, Y., Boue, F., Joanicot, M. & Cabane, B. (1996). Macromolecules, 29, 4346-4359.]; Clement et al., 2001[Clement, F., Bokobza, L. & Monnerie, L. (2001). Rubber Chem. Technol.  74, 847-870.]; Kishimoto et al., 2006[Kishimoto, H., Shinohara, Y., Suzuki, Y., Takeuchi, A., Uesugi, K., Yagi, N., Muraoka, K., Mizoguchi, T. & Amemiya, Y. (2006). XIIIth International Conference on Small-Angle Scattering, 9-13 July, Kyoto, Japan.]; Morfin et al., 2006[Morfin, I., Ehrburger-Dolle, F., Grillo, I., Livet, F. & Bley, F. (2006). J. Synchrotron Rad. 13, 445-452.]; Harrak et al., 2006[Harrak, A. E., Carrot, G., Jestin, J., Oberdisse, J. & Boue, F. (2006). XIIIth International Conference on Small-Angle Scattering, 9-13 July, Kyoto, Japan.]), active simulations (Oberdisse et al., 2000[Oberdisse, J., Rharbi, Y. & Boue, F. (2000). Comput. Theor. Polym. Sci. 10, 207-217.]) were also conducted by changing the geometry, phase hardness and degree of aggregation of nanoparticles in the composites, where the experimental results by SANS, small-angle X-ray scattering (SAXS), ultra-small-angle neutron scattering (USANS), ultra-small-angle X-ray scattering (USAXS) and atomic force microscopy (AFM) were utilized. Several of the samples in these studies, however, were the nanocomposites in which the nanoparticles seem to be aggregated in the matrixes. Thus, our study is to conduct time-resolved experiments under the fast deformation of the soft nanocomposites in which there was well dispersed in situ generated particulate silica.

2. Experimental

2.1. Materials

Peroxide-crosslinked isoprene rubber was prepared as follows: 100 g of isoprene rubber (IR, JSR IR-2200) was mixed with one gram of dicumyl peroxide (i.e. 1 phr in terms of parts per hundred rubber by weight) on a two-roll mill. The mix was cured under a heat-pressing at 428 K for 30 min in a mold to give a crosslinked IR sheet of 1 mm thickness. In situ silica filling was carried out by the sol–gel reaction of TEOS in the crosslinked IR matrix. The crosslinked IR sheet was immersed in TEOS for 24 h at 313 K. The swollen IR sheet was then immersed in 2 wt% aqueous solution of n-butylamine at 323 K for 48 h to conduct the sol–gel reaction of TEOS. The sample was dried under vacuum at 323 K for 48 h. The in situ silica content was 9.7 vol% (22 phr), which was determined by thermogravimetric analysis (Rigaku TG). The network-chain density of the sample was 1.0 × 10−4 mol cm−3 which was determined by a microcompression method (Flory, 1953[Flory, P. J. (1953). Principles of Polymer Chemistry. Ithaca: Cornell University Press.]; Smith, 1969[Smith, D. (1969). Rubber Chem. Technol. 42, 580-588.]) using a Thermo-Mechanical Analyzer (TG-50TMA of Shimadzu Co.). Ring-shaped specimens were cut out from the in situ silica filled sample, with inner and outer diameters of 11.7 and 13.7 mm, respectively.

2.2. Transmission electron microscopy

Ultra-thin film of the sample was prepared using a microtome (MT-XL Ultramicrotome, Boeckeler Instrument, Inc.) in liquid nitrogen. The specimen was placed on a copper grid which was coated in advance with Folmvar and evaporated carbon. Then, a transmission electron microscopy (TEM) observation was carried out with a transmission electron microscope (Jeol TEM-100U). The accelerating voltage was 80 kV.

2.3. Simultaneous small-angle X-ray scattering and tensile measurement

Synchrotron SAXS measurements were carried out on the BL-40B2 beamline at SPring-8, Harima, Japan (https://www.spring8.or.jp/j/ ). A special-made tensile tester (with cooperation of Aiesu Giken Co., Kyoto) was placed on the beamline. During the tensile measurement at room temperature (ca 298 K), SAXS patterns were recorded simultaneously. The wavelength of the X-ray was 0.15 nm and the camera length was 3 m. Two-dimensional SAXS patterns were recorded using CCD camera (Hamamatsu C4880-00). The incident beam was exposed at every 6 s for 50 ms in order to avoid radiation damage of the specimen. Using the tensile tester, the specimen could be stretched symmetrically to be irradiated at almost the same position of the specimen by X-ray. The ring-shaped sample was used to correctly measure the elongation ratio (α) of the deformed sample. Here, α is defined as α = l/l0, in which l0 is the initial length and l is the length after deformation. The stretching and retracting speeds were 100 mm min−1, i.e. strain speed was 5 s−1.

3. Results and discussion

Fig. 1[link] shows a TEM photograph of the in situ silica filled soft nanocomposite, the silica content of which was 9.7 vol%. In situ generated silica particles in the peroxide-crosslinked IR matrix were spherical. The average diameter of the in situ silica particles was ca 34 nm and its distribution was very narrow. Also, the dispersion of the particles in the rubber matrix was random, i.e. very homogeneous. The distance between the silica particles was calculated to be ca 72 nm. The sol–gel reaction of TEOS was found to produce very fine and homogeneous silica particles in the IR network. Therefore, this nanocomposite is most preferable as a model for investigating the deformation behavior of nanofillers in soft materials.

[Figure 1]
Figure 1
TEM photograph of the in situ silica filled IR nanocomposite.

Tensile stress-elongation ratio curve of the nanocomposite is illustrated in Fig. 2[link] and simultaneously obtained two-dimensional SAXS patterns are shown in Fig. 3[link]. In each SAXS pattern, the number inside shows the elongation ratio and `re' means the retracting process. The SAXS patterns beyond α = 2.5 and α = re3 under the stretching and retracting processes, respectively, were not subjected to the analysis due to the over-running of detectable range of scattering peaks under the present experimental conditions. As shown in Fig. 3[link](a), an isotropic pattern was observed before stretching, which may imply that the silica particles were randomly dispersed in the rubber matrix before stretching. This was fully in accord with the TEM result in Fig. 1[link]. The estimated average spacing between the silica particles, d, was ca 73 nm, where d was calculated by d = 2π/q. This equation is derived from q = 4πsin(θ/2)/λ and the Bragg equation. q is the magnitude of scattering vector, θ is the scattering angle and λ is the wavelength of the X-rays. The obtained value was in good agreement with that obtained by TEM.

[Figure 2]
Figure 2
Stress–elongation ratio curve of the in situ silica filled IR nanocomposite.
[Figure 3]
Figure 3
Two-dimensional SAXS patterns of the in situ silica filled IR nanocomposite during tensile deformation.

By stretching the sample to α = 1.5, the ring-shaped two-dimensional SAXS pattern was changed to the pattern shown in Fig. 3[link](b), where the meridional scattering increased and equatorial scattering significantly decreased. It was not a butterfly pattern, which was detected by stretching of carbon black filled styrene–butadiene vulcanizate by Morfin et al. (2006)[Morfin, I., Ehrburger-Dolle, F., Grillo, I., Livet, F. & Bley, F. (2006). J. Synchrotron Rad. 13, 445-452.], for example. It is worth noting that a similar two-dimensional SAXS pattern with our result was obtained by a computer simulation for a soft nanocomposite by Rharbi et al. (1999)[Rharbi, Y., Cabane, B., Vacher, A., Joanicot, M. & Boue, F. (1999). Europhys. Lett. 46, 472-478.]. The simulation was conducted as follows: hard sphere particles were placed at random in a box that represented the polymer matrix, then the box was stretched in the parallel direction and compressed in the perpendicular direction and the centers of mass of the particles were displaced affinely in accord with the macroscopic deformation. Applying these mechanisms to our nanocomposite, we can deduce that upon deformation the internal stress forces the silica particles to come close together in the perpendicular direction and to separate in the parallel direction against the stretching direction, respectively. Consequently, the morphology shown in Fig. 4[link](b) of in situ silica particles is speculated to be formed at α = 1.5. Recently, we clarified that the network structure of peroxide-crosslinked natural rubber was more homogeneous compared with that of the sulfur-cured one, by studying their strain-induced crystallization behavior using simultaneous tensile and synchrotron wide-angle X-ray diffraction measurements (Ikeda et al., 2007[Ikeda, Y., Yasuda, Y., Makino, S., Yamamoto, S., Tosaka, M., Senoo, K. & Kohjiya, S. (2007). Polymer, 48, 1171-1175.]). Therefore, the in situ silica particles generated in the peroxide-crosslinked IR network must be placed at random without a maldistribution in the rubber matrix. This characteristic is considered to give the two-dimensional SAXS pattern shown in Fig. 3[link](b) in agreement with the simulation result.

[Figure 4]
Figure 4
Speculated morphological change of silica particles in the in situ silica filled IR nanocomposite upon deformation.

By further stretching to α = 2, the two-dimensional SAXS pattern evolved into a set of four maxima as shown in Fig. 3[link](c), although the intensity scale makes it difficult to see the maxima. This observation is considered to suggest the formation of a buckling structure of silica particles by stretching. Our AFM observation supported this consideration (not shown here). This morphological change of in situ silica particles is ascribable to the elongation in the stretching direction and the compression from the lateral directions occurring simultaneously during uniaxial stretching. On the appearance of a four-spot pattern, Rharbi et al. (1999)[Rharbi, Y., Cabane, B., Vacher, A., Joanicot, M. & Boue, F. (1999). Europhys. Lett. 46, 472-478.] proposed two processes; either some long aggregates buckle under the lateral compression, or the space in the perpendicular direction to the stretching between two aggregates is filled up by another aggregate that forced between them. For the moment, we can not clarify the mechanism of buckling for our nanocomposite. However, the four-spot pattern obtained was very similar to the computer simulated one on the basis of the shear displacement model by Rharbi et al. (1999)[Rharbi, Y., Cabane, B., Vacher, A., Joanicot, M. & Boue, F. (1999). Europhys. Lett. 46, 472-478.]. Thus, the latter phenomenon can be ascribed to the deformation mechanism for our in situ silica filled nanocomposite. From the consideration mentioned above, the estimated morphological change of in situ silica particles in the IR network is illustrated in Fig. 4[link]. It is a very simplified image to understand and the real model may be less organized. Further time-resolved SAXS measurement is necessary for clarifying the phenomenon.

In this study, the four-spot pattern to show the buckling structure of in situ silica particles was clearly detected during the retracting process as shown in Fig. 3[link](d)–(g). The spacing between the silica layers decreased upon retracting. Moreover, the degree of buckling to the stretching direction in the retracting process became smaller with the decrease of strain, which was ascribed to the releasing the compression from the lateral directions. The buckling structure was also found to partially remain when the sample was retracted to α = 1 at the retracting speeds of 100 mm min−1.

The distance between the silica layers along the stretching direction (D) was calculated by using an equation of D = d/cos μ, where μ is the azimuthal angle of the four-spot pattern as shown in Fig. 3[link]. Using the D values at each deformation, the microscopic elongation ratio was calculated and plotted against the macroscopic elongation ratio measured by the simultaneous tensile measurement in Fig. 5[link]. Interestingly, a good linearity was observed between them, which suggests the affine deformation of the in situ silica filled soft nanocomposite. It should be kept in mind, however, that the silica particles are undeformable and consequently the crosslinked IR matrix of the nanocomposite must be deformed non-affinely to the macroscopic deformation.

[Figure 5]
Figure 5
Relationship between the microscopic and macroscopic elongation ratios of the in situ silica filled IR nanocomposite.

4. Conclusion

The morphological change of the in situ silica particles, which were generated in the IR network with a fairly homogeneous dispersion, was investigated during the deformation by two-dimensional SAXS and simultaneous tensile measurements. The morphology of in situ silica particles became the buckling structure from the random state by elongating to the stretching direction and compressing from the lateral directions during uniaxial stretching. These observed morphological changes were in good agreement with those of the simulation on the basis of the displacement model by Rharbi et al. (1999)[Rharbi, Y., Cabane, B., Vacher, A., Joanicot, M. & Boue, F. (1999). Europhys. Lett. 46, 472-478.]. The buckling structure of silica particles was clearly observed during the retracting process. The affine deformation of this nanocomposite was detected at low strain. USAXS or USANS results are required to elucidate the deformation behavior of in situ silica particles further up to the larger deformation.

Acknowledgements

The synchrotron radiation experiment was performed on the BL-40B2 beamline at SPring-8 with the approval of the Japan Synchrotron Radiation Research Institute (JASRI) (Proposal Nos 2005B0661-NL2b-np and 2006A1298-NL2b-np). This work was supported by the Research Grants from President of KIT 2005 & 2006.

References

First citationBrinker, C. J. & Scherer, G. W. (1982). Sol–Gel Science. New York: Academic Press.
First citationClement, F., Bokobza, L. & Monnerie, L. (2001). Rubber Chem. Technol. 74, 847–870. CAS
First citationFlory, P. J. (1953). Principles of Polymer Chemistry. Ithaca: Cornell University Press.
First citationHarrak, A. E., Carrot, G., Jestin, J., Oberdisse, J. & Boue, F. (2006). XIIIth International Conference on Small-Angle Scattering, 9–13 July, Kyoto, Japan.
First citationIkeda, Y., Yasuda, Y., Makino, S., Yamamoto, S., Tosaka, M., Senoo, K. & Kohjiya, S. (2007). Polymer, 48, 1171–1175. Web of Science CrossRef CAS
First citationKishimoto, H., Shinohara, Y., Suzuki, Y., Takeuchi, A., Uesugi, K., Yagi, N., Muraoka, K., Mizoguchi, T. & Amemiya, Y. (2006). XIIIth International Conference on Small-Angle Scattering, 9–13 July, Kyoto, Japan.
First citationKohjiya, S. & Ikeda, Y. (2000). Rubber Chem. Technol. 73, 534–550. CrossRef CAS
First citationKohjiya, S., Yajima, A., Yoon, J. R. & Ikeda, Y. (1994). Nippon Gomu Kyokaishi, 67, 859–861. CrossRef CAS
First citationKraus, G. (1965). Reinforcement of Elastomers. New York: Interscience.
First citationMark, J. E. (1985). Science of Ceramic Chemical Processing, edited by L. L. Hench & R. D. Ulrich, ch. 47. New York: John Wiley & Sons.
First citationMark, J. E. & Pan, S.-J. (1982). Macromol. Chem. Rapid Commun. 3, 681–685. CrossRef CAS
First citationMorfin, I., Ehrburger-Dolle, F., Grillo, I., Livet, F. & Bley, F. (2006). J. Synchrotron Rad. 13, 445–452. Web of Science CrossRef CAS IUCr Journals
First citationOberdisse, J., Rharbi, Y. & Boue, F. (2000). Comput. Theor. Polym. Sci. 10, 207–217. Web of Science CrossRef CAS
First citationRharbi, Y., Boue, F., Joanicot, M. & Cabane, B. (1996). Macromolecules, 29, 4346–4359. CrossRef CAS Web of Science
First citationRharbi, Y., Cabane, B., Vacher, A., Joanicot, M. & Boue, F. (1999). Europhys. Lett. 46, 472–478. Web of Science CrossRef CAS
First citationSmith, D. (1969). Rubber Chem. Technol. 42, 580–588.  CrossRef

© International Union of Crystallography. Prior permission is not required to reproduce short quotations, tables and figures from this article, provided the original authors and source are cited. For more information, click here.

Journal logoJOURNAL OF
APPLIED
CRYSTALLOGRAPHY
ISSN: 1600-5767
Follow J. Appl. Cryst.
Sign up for e-alerts
Follow J. Appl. Cryst. on Twitter
Follow us on facebook
Sign up for RSS feeds