research papers
Multilateral surface analysis of the CeB6 electron-gun cathode used at SACLA XFEL
aJapan Synchrotron Radiation Research Institute, Kouto, Sayo, Hyogo 679-5198, Japan, and bRIKEN SPring-8 Center, Kouto, Sayo, Hyogo 679-5148, Japan
*Correspondence e-mail: o-taku@spring8.or.jp
The CeB6(001) single crystal used as a cathode in a low-emittance electron gun and operated at the free-electron laser facility SACLA was investigated using cathode lens combined with at SPring-8 synchrotron radiation facility. Multilateral analysis using thermionic emission low-energy ultraviolet and X-ray photoemission and hard X-ray photoemission spectroscopy revealed that the thermionic electrons are emitted strongly and evenly from the CeB6 surface after pre-activation treatment (annealing at 1500°C for >1 h) and that the thermionic emission intensity as well as elemental composition vary between the central area and the edge of the old CeB6 surface.
Keywords: thermally activated processes; photoemission; synchrotron radiation; microstructures; CeB6; LEEM; PEEM; TEEM; thermionic electron cathode.
1. Introduction
SACLA (SPring-8 Angstrom Compact free-electron LAser), the X-ray free-electron laser (XFEL) facility in Japan (Ishikawa et al., 2012), boasts a compact body which is attained by an in-vacuum undulator system and extremely stable laser pulse emission. Instead of using a photocathode, which is popular at XFEL facilities worldwide, a thermionic electron cathode is used to provide low-emittance electron beams of high stability over a long duration. The CeB6(001) single-crystal cathode with ∼3 mm diameter is activated by heating to ∼1500°C and an initial electron beam with a beam energy of 500 keV, of 1 A, pulse width of 3 µs, repetition rate of 60 Hz and normalized emittance of ∼0.6 mm mrad (r.m.s.) have been provided routinely (Togawa et al., 2007). Nevertheless, the degradation of the emission power over a very long term operation is still unavoidable; initially, the cathode can emit over ∼1 A at only 1450°C, then it gradually requires increasing of the temperature to maintain its emission level, and finally is unable to emit 1 A even if it is heated thoroughly to 1550–1600°C. The cathodes have been changed about once a year, so determining the cause of cathode degradation is critical for more reliable beam activity.
Meanwhile, a cathode lens microscope, specifically the spectroscopic photoemission and low-energy electron microscope (SPELEEM) combined with synchrotron radiation (SR) X-rays, is a powerful instrument for studying the physical and chemical properties of the thermionic cathode materials at both microscopic and macroscopic levels. Low-energy ; Bauer, 2019), photoemission (PEEM) and other forms of electron emission microscopy are among the observation modes available in SPELEEM. In the LEEM mode, an incident electron beam with minus few tens of kV of acceleration voltage (EHV) is decelerated at a sample biased at EHV + ESTV (in which a start voltage ESTV is typically 0–50 V), i.e. the effective incident electron energy (ESTV) is low and thus the generated electron image represents well the surface electronic states of the sample. Different kinds of electrons like the reflected, inelastically scattered, Auger and can be visualized selectively by choosing appropriate ESTV. By changing the lens parameters to reciprocal-space imaging mode, patterns can be obtained. However, lights rather than electron beams are used as photoemission excitation sources in the PEEM mode. Ultraviolet (UV) lights are used to obtain the spatial distribution of functions of materials, while synchrotron radiation X-rays help to visualize information equivalent to X-ray magnetic circular/linear dichroism (XMCD/XMLD), X-ray photoemission spectroscopy, and so on. Besides the functions of LEEM and PEEM as explained above, the SPELEEM can project other types of electrons emitted from the specimen. For instance, field emission electrons emitted from irregular or sharpened material surfaces by applying a strong electric field are regarded as an undesirable background for LEEM/PEEM observations, while thermionic emission electrons, derived from materials with low work functions under high temperature, can be a good object for microscopic investigations of thermionic cathode materials. Though the possibility of thermionic emission-electron microscopy (TEEM) has been mentioned since the beginning of the instrumental development of cathode lens microscopy (Bauer, 1994), there have been few reports on TEEM observations (Fukidome et al., 2006; Lu et al., 2018, 2020).
(LEEM) (Telieps & Bauer, 1985In this study, we report on surface-state investigations of CeB6(001) single-crystal ingots used as an electron-gun cathode at SACLA. TEEM observations of a pristine CeB6 sample (having the same shape as the CeB6 used in SACLA) revealed that the initial 1500°C annealing was necessary to remove a surface-oxidized layer and to exert a good emission power evenly over the entire surface. We also discovered that thermionic emissions were more significant at the step edges rather than at the flat terraces in the purified (annealed) surface. Control experiments between pristine and used (employed in SACLA for ∼1 year) CeB6 by TEEM, LEEM, UV and X-ray PEEM (UV-PEEM and X-PEEM) and hard X-ray photoemission spectroscopy (HAXPES) revealed that the long period operation causes inhomogeneity in the elemental composition, and the thermionic electron emission power on the CeB6 surface between the center and the edge and possible origins are discussed.
2. Experimental
The samples used in this study were commercial CeB6(001) single-crystal ingots (APTech Inc., USA) of ∼3 mm diameter and 5 mm length with mirror-polished surfaces [Fig. 1(a)]. Microscopic measurements were performed using a SPELEEM apparatus [LEEM III with imaging energy analyzer (ELMITEC GmbH)] (Guo et al., 2007) incorporated at the BL17SU soft X-ray beamline at SPring-8 (Ohashi et al., 2007; Senba et al., 2007) with which LEEM, UV-PEEM, X-PEEM (and XAS) and TEEM observations are available in the same field-of-view (FOV). Photon and electron sources used in these observations were: LEEM — electron beam (LaB6, −20 kV); UV-PEEM — high-pressure mercury lamp; and X-PEEM — soft X-rays produced from a multi-polarization-mode undulator (Shirasawa et al., 2004). Meanwhile, without using any external sources, TEEM images were obtained by simply heating the sample to 1000–1200°C. The sample was mounted on an ELMITEC standard sample holder, which can withstand temperatures up to ∼1200°C (∼2000°C for short flashing). For macroscopic chemical analysis, we used a HAXPES apparatus (Woicik, 2016; Ikenaga et al., 2013) installed at the BL47XU hard X-ray beamline and systematically investigated the composition variation in the CeB6 from the point of view of the position-dependence of core-electron peaks' intensities of the constituent elements. A size of the beam footprint on the sample for the HAXPES measurement was 0.04 mm (w) × 1 mm (h), where w and h correspond to the directions that are parallel and perpendicular to the scanning direction, respectively. Approximate probing depths are less than 1 nm for LEEM, several nanometres for PEEM and TEEM, and several tens of nanometres for HAXPES.
3. Results and discussion
Figs. 1(c), 1(d) and 1(e), respectively, show LEEM, UV-PEEM and TEEM images (diameter of FOV: 75 µm) of a pristine CeB6(001) single crystal at the representative positions shown in Fig. 1(b) (note that the grayscale of the images is different for each condition). Due to mechanical and thermal drift, at the same (nominal) distance from the center, slight differences in the measurement position between different measurement conditions are noted [the same is true for Figs. 3 and Fig. 4(b) shown later]. Two dark stain-like patterns (exemplified by a red dotted circle) are unwanted burned areas of the micro-channel plate (MCP) caused by thermionic emission electron's overexposure. The LEEM and PEEM images are taken at room temperature (RT) before and after annealing at 1500°C for about an hour (in situ at the main experimental chamber). The LEEM images shown in Fig. 1(c) are obtained with ESTV set to ∼0 V, which corresponds to surface topology observations [so-called mirror (MEM)]. The annealing process flattens out the rough surface with some scratches (e.g. a large ditch-like structure found at 0 mm). A similar tendency can be found from the UV-PEEM images in Fig. 1(d). Furthermore, annealing significantly improved the overall PEEM image intensity, presumably due to the reduction of the oxidized surface (note that the number of photoemission electrons at the UV range well reflects the function). The temperature dependence of the TEEM image intensities [Fig. 1(e)] also follows the trend of the UV-PEEM results, that is, the thermionic emission is sporadic for all observed temperatures (1000 and 1200°C) before the 1500°C annealing but it becomes homogeneous after annealing. Although the TEEM observations were planned to be performed at temperatures up to ∼1500°C, i.e. similar temperature as the SACLA operation, the electron emission at that temperature reaches as high as ∼1 A, which far exceeds the interlock limit of the SPELEEM's objective lens (∼130 mA). Therefore, we decided to obtain images within 1000–1200°C, although the annealing treatment up to ∼1500°C was performed in situ in the main observation chamber with EHV turned off. We confirmed that the TEEM contrast after annealing [third and fourth rows of Fig. 1(e)] is analogous between 1000°C and 1100°C for all the positions and hence the suppressed observation temperature may not affect qualitative discussion. The temperature-dependence of the TEEM image intensity averaged over all the observed areas is shown in Fig. 1(f) [blue markers and arrows for pristine CeB6; details of the results for used CeB6 (red markers and arrows) are explained later]. The unit of intensity values is arbitrary but unified for all LEEM/PEEM/TEEM observations in this article, by calibrating with the amplification rates determined by MCP voltages. At the initial heating process, dramatic increases of the thermionic emission by approximately one and two orders of magnitude for 1000°C → 1100°C and 1100°C → 1200°C, respectively, are observed. As for the effect of 1500°C annealing, the thermionic emission is improved by approximately one order of magnitude after annealing, according to the comparison at the same temperature (e.g. 2.8 and 40 at 1000°C before and after annealing, respectively).
XAS spectra of pristine CeB6 at the Ce M4,5-, B K- and O K-absorption edges were drawn by extracting X-PEEM image intensities with sweeping photon energies across the absorption edges, as shown in Fig. 2 (representative X-PEEM images for Ce M4,5- and B K-edges are shown later in Fig. 8). The temperature for X-PEEM observations (∼600°C) is low enough to remove the thermionic electron emission but high enough to prevent synchrotron radiation irradiation from contaminating the sample. The spectral shape after annealing (red line) in the Ce M5-edge region [Fig. 2(a)] shows a double-peak structure, which is typical for the Ce3+ state (Mitra et al., 2003) and is similar to the previously reported spectral shape of CeB6 (Magnuson et al., 2001). The surface chemical state seems to remain unchanged since the overall shape of the Ce M4,5-edge spectrum does not change by the annealing. However, it does not rule out the possibility that cerium oxide existed before annealing because the cerium is trivalent also in Ce2O3. In fact, the spectral change in the B K-edge region is striking, as shown in Fig. 2(b). The sharp peak observed at 193.6 eV before annealing (blue arrow) was greatly suppressed after annealing. We consider that this peak originates from boron oxide because the reported B K-edge spectrum of B2O3 showed a similar sharp peak around 194 eV (Gilbert et al., 2000). We also verified substantial suppression of the absorption structure around the O K-edge [Fig. 2(c)]. From these results, we conclude that the enhancement of the electron emission observed in the UV-PEEM and TEEM results in Figs. 1(d) and 1(e) is associated with the reduction of the surface oxide.
Fig. 3(a) shows magnified LEEM (600°C) and TEEM (1000°C) images (diameter of FOV: 15 µm) taken at the center of the pristine CeB6 after the annealing process. A fine but clear step-and-terrace structure is recognized from the LEEM image. Although the fine structure in the TEEM image is similar to that in the LEEM image, the intensity contrast is opposite; thermionic emission is more significant from the step edges than from the flat terraces. The result is convincing, considering the general fact that the field emission electrons are salient around sharpened edges. Note that no field emission electrons are recognized under the LEEM/PEEM observations at RT. Fig. 3(b) shows similar images as Fig. 3(a) taken for a CeB6(001) ingot, which had operated as the electron-gun cathode at SACLA for about a year (we refer to this sample as `used CeB6' hereafter). This sample does not show a clear step-and-terrace pattern as found in the pristine one but the surface roughness (<100 nm) is still low enough to provide a low-emittance beam required at SACLA.
Fig. 4(b) shows position-dependent TEEM images of the used CeB6(001) taken at 1000°C before and after the 1500°C annealing for ∼1 h [image acquisition points are shown by red dots in Fig. 4(a)]. The full profile of the TEEM, LEEM and UV-PEEM images is shown in Figs. SM1 and SM2 of the supporting information [image acquisition points are indicated by red and gray dots in Fig. 4(a)]. The chemical and electron emission properties of CeB6 may be anisotropic, based on the shape and position of the sleeves of the graphite heater used to heat it during the SACLA process [see schematic drawing in Fig. 4(a)]. The probing direction which includes and excludes the points of contact with the carbon sleeves is `45°' and `0°', respectively. The surface of the used CeB6 [Fig. 4(b)] is slightly rougher than that of pristine CeB6 before annealing [Fig. 1(e)]. The roughness is mostly wiped out by annealing treatment, though some prominent defects remain. The temperature dependence of the average TEEM intensity of the used CeB6 is shown in Fig. 1(f) with red markers and arrows. Although the thermionic emission is improved by annealing, the increment is not very dramatic as in the case of the pristine CeB6 (blue plots), suggesting that the oxidized layer formed by exposure to the air (existing before annealing) is not so thick for the used CeB6 surface as for the pristine surface, due to the long-period activation in SACLA. Meanwhile, the intensity at 1000°C after annealing is lower for pristine CeB6 (40.7) than for used CeB6 (1074), being incompatible with the fact that the emission power has deteriorated over a long-period operation. Although the reason for this result is unclear, we believe that the annealing condition in this experiment did not accurately represent the actual operation condition in SACLA, i.e. the annealing time of ∼1 h at 1500°C was insufficient to thoroughly purify the virgin CeB6 surface and obtain maximum emission power (the actual cathode is continuously heated about 1500°C during SACLA operation). In fact, the absorption fine structure at the oxygen K-edge is not completely eliminated by the ∼1 h annealing [Fig. 2(c)]. Note that since the limit of continuous heating of the SPELEEM manipulator is supposed to be up to ∼1200°C, we must give up further annealing for fear of damaging the insulating ceramics in the manipulator.
The sample position and scanning azimuth dependence of TEEM (1000°C) and UV-PEEM (RT) image intensity of used CeB6 after annealing is summarized in Fig. 5. The TEEM image intensity [Fig. 5(a)] is significantly higher around the edges than around the center. Although this tendency may partly be attributed to extrinsic factors such as an inhomogeneous temperature within the ingot surface, we assume that it is mainly derived from the variation of functions, since the profile of UV-PEEM intensities [Fig. 5(b)] measured at RT show a similar tendency.
For comparison, Fig. 6 shows an example of a HAXPES spectrum [hν = 7.94 keV, center of ingot, Fig. 6(a)] and position-dependence (0° direction) of the Ce 4p, B 1s and C 1s peak intensities [Fig. 6(b)] of used CeB6 obtained at RT. Note that the annealing procedure was not performed due to the HAXPES experimental station's instrument limitation. The B 1s and Ce 4p peaks abruptly decrease around the edge of the ingot while the C 1s peak increases, suggesting that the surface is contaminated by the carbon sleeve or the boron atoms are partially replaced by the carbon atoms. However, thermionic electrons are rather enhanced around the edge of used CeB6 [Fig. 5(a)]. Furthermore, the overall shapes of the intensity profiles are similar between C/Ce [inset of Fig. 6(b)], TEEM [Fig. 5(a)] and UV-PEEM [Fig. 5(b)], and the tendency of the TEEM intensity profile is not so different between the 0° and 45° directions. Therefore, it seems that the carbon impurity does not significantly contribute to the degradation of the electron emission power but rather contributes to the suppression of the degradation. Another possible factor of the age-related deterioration is a compositional deviation from CeB6 by long-period hard heating, which may occur on the entire surface. The chemical bond of the cerium atoms buried in the center of the B6 network with firm is relatively weak, causing the cerium atoms to be preferentially evaporated at the thermal-excitation state (Gurin et al., 2001).
Fig. 7 shows the ESTV dependence of UV-PEEM image intensities for pristine and used CeB6 samples obtained at RT after the annealing, as indirect evidence of compositional change (Ce evaporation) over the long SACLA operation [for images at representative ESTV (see Fig. SM3 of the supporting information)]. In PEEM observations, ESTV corresponds to the energy of that go through the energy slit at the exit of the electron analyzer (energy resolution ΔE ≃ 1 eV). In our LEEM apparatus, the intensity peak should be observed around ESTV = 1–2 V, taking into account the work function of CeB6 (∼2.6 eV) (Lafferty, 1951). While the pristine CeB6 (blue line) shows the expected result, the ESTV peak of the used CeB6 (red line) shows an unusual value of ∼0 V. Additionally, the image intensity is unstable, as shown by the noisy or spiky intensity curve for the used CeB6 (red line). These results suggest the charging of the surface of the used CeB6. Note that the ESTV dependence in Fig. 7 was not measured near the ingot edge, where the carbon contamination was prominent, but around the center of the CeB6 surface. CeB6 has good (the order of 10 µΩ cm) (Greiner & Gutowski, 1957), while pure boron is a semi-metal whose resistivity is of the order of 1–10 MΩ cm at RT (Tanaka et al., 1980). Considering that the of boron-based materials is sensitive to their chemical states, the observed charging behavior supports the possibility that a more salient increase of the B 1s peak than its Ce 4f counterpart (i.e. larger B/Ce ratio) around the center of the cathode seen in Fig. 6(b) is caused by the compositional deviation from CeB6; cerium is poorly contained on the used CeB6 surface.
Meanwhile, the X-PEEM result revealed no compositional inhomogeneity on a microscopic scale. Fig. 8 shows surface chemical contrast maps of the pristine and used CeB6 samples obtained by taking the X-PEEM images around the Ce M5- and B K-edges (after annealing, ∼600°C). The element contrast maps are obtained by dividing the image obtained at the peak top energy of the corresponding by that obtained at the pre-edge region [examples of full spectra around Ce M5- and B K-edges are shown in Figs. 2(a) and 2(b), respectively]. The imaging areas are identical to those shown in Figs. 3(a) and 3(b) for pristine and used samples, respectively. Note that B K-edge images of used CeB6 were unavailable, since the low photon energy region (<450 eV) was inaccessible at that time due to an accident in the insertion device of BL17SU. The image contrast, seen both in the peak (887.2 eV) and pre-edge (881.0 eV) energies around the Ce M5-edge of pristine CeB6 [Fig. 8(a)], which is analogous to that found in the TEEM image [Fig. 3(a)], disappeared in the element contrast image (peak/pre). This indicates that the contrast seen in the raw X-PEEM images (at peak and pre-edge) is not derived from chemical inhomogeneity but from any other factors such as topological unevenness, defects and contamination by other elements. The same tendency is also seen in the elemental contrast image around the B K-edge of pristine CeB6 [Fig. 8(b)] and around the Ce M5-edge of used CeB6 [Fig. 8(c)], i.e. there is practically no chemical inhomogeneity when observed microscopically, even in the used CeB6. Therefore, we conclude that, if the preferential evaporation of the cerium atoms was occurring during the thermionic emission, the Ce atoms were evaporated evenly.
4. Conclusion
In conclusion, we implemented a multilateral surface analysis of CeB6(001) single crystals used as the electron-gun cathode at SACLA XFEL, using TEEM, LEEM, UV-PEEM, X-PEEM and HAXPES. The TEEM observations revealed that homogeneous and strong electron emission power was exerted after annealing treatment up to ∼1500°C and that the annealed surface of the pristine CeB6 showed a step-and-terrace structure in which the step edges emitted stronger thermionic electrons than flat terraces. Through further analysis including X-rays spectroscopy we found an increase in the electron emission as well as a variation in the elemental composition around the edge of the used CeB6 cathode. Even though the discussion based on the possible reasons, carbon influx and preferential evaporation of the cerium has not been conclusive, the findings in this study significantly push the project, i.e. development of the viable cathode, to the ultimate goal, as well as show the strength of the cathode lens microscopy combined with synchrotron radiation spectroscopy as a tool to investigate the surface of thermionic emission-electron materials.
Supporting information
SM1,2. Full profile of LEEM, UV-PEEM and TEEM images of used CeB6 along 0° (SM1) and 45° (SM2) direction. SM3. E_STV-dependent UV-PEEM images of pristine and used CeB6. DOI: https://doi.org/10.1107/S1600577521009656/ok5053sup1.pdf
Acknowledgements
The experiments at SPring-8 were performed with the approval of the Japan Synchrotron Radiation Research Institute (Proposal Nos. 2016A1317 (BL17SU) and 2016B1446 (BL47XU)) and RIKEN SPring-8 Center (Proposal Nos. 20190060 (BL17SU), 20200037 (BL17SU)). TO thanks Enago (https://www.enago.jp) for the English language review.
References
Bauer, E. (1994). Rep. Prog. Phys. 57, 895–938. CrossRef CAS Web of Science Google Scholar
Bauer, E. (2019). Handbook of Microscopy, edited by P. W. Hawkes & J. C. H. Spence, pp. 487–535. Springer. Google Scholar
Fukidome, H., Yoshimura, M. & Ueda, K. (2006). Jpn. J. Appl. Phys. 45, 70–72. Web of Science CrossRef CAS Google Scholar
Gilbert, B., Perfetti, L., Fauchoux, O., Redondo, J., Baudat, P., Andres, R., Neumann, M., Steen, S., Gabel, D., Mercanti, D., Ciotti, M. T., Perfetti, P., Margaritondo, G. & De Stasio, G. (2000). Phys. Rev. E, 62, 1110–1118. Web of Science CrossRef CAS Google Scholar
Greiner, E. S. & Gutowski, J. A. (1957). J. Appl. Phys. 28, 1364–1365. CrossRef CAS Web of Science Google Scholar
Guo, F. Z., Muro, T., Matsushita, T., Wakita, T., Ohashi, H., Senba, Y., Kinoshita, T., Kobayashi, K., Saitoh, Y., Koshikawa, T., Yasue, T., Oura, M., Takeuchi, T. & Shin, S. (2007). Rev. Sci. Instrum. 78, 066107. Web of Science CrossRef PubMed Google Scholar
Gurin, V. N., Korsukova, M. M., Loginov, M. V. & Shrednik, V. N. (2001). Tech. Phys. Lett. 27, 431–433. Web of Science CrossRef CAS Google Scholar
Ohashi, H., Senba, Y., Kishimoto, H., Miura, T., Ishiguro, E., Takeuchi, T., Oura, M., Shirasawa, K., Tanaka, T., Takeuchi, M., Takeshita, K., Goto, S., Takahashi, S., Aoyagi, H., Sano, M., Furukawa, Y., Ohata, T., Matsushita, T., Ishizawa, Y., Taniguchi, S., Asano, Y., Harada, Y., Tokushima, T., Horiba, K., Kitamura, H., Ishikawa, T. & Shin, S. (2007). AIP Conf. Proc. 879, 523–526. CrossRef CAS Google Scholar
Ikenaga, E., Kobata, M., Matsuda, H., Sugiyama, T., Daimon, H. & Kobayashi, K. (2013). J. Electron Spectrosc. Relat. Phenom. 190, 180–187. Web of Science CrossRef CAS Google Scholar
Ishikawa, T., Aoyagi, H., Asaka, T., Asano, Y., Azumi, N., Bizen, T., Ego, H., Fukami, K., Fukui, T., Furukawa, Y., Goto, S., Hanaki, H., Hara, T., Hasegawa, T., Hatsui, T., Higashiya, A., Hirono, T., Hosoda, N., Ishii, M., Inagaki, T., Inubushi, Y., Itoga, T., Joti, Y., Kago, M., Kameshima, T., Kimura, H., Kirihara, Y., Kiyomichi, A., Kobayashi, T., Kondo, C., Kudo, T., Maesaka, H., Maréchal, X. M., Masuda, T., Matsubara, S., Matsumoto, T., Matsushita, T., Matsui, S., Nagasono, M., Nariyama, N., Ohashi, H., Ohata, T., Ohshima, T., Ono, S., Otake, Y., Saji, C., Sakurai, T., Sato, T., Sawada, K., Seike, T., Shirasawa, K., Sugimoto, T., Suzuki, S., Takahashi, S., Takebe, H., Takeshita, K., Tamasaku, K., Tanaka, H., Tanaka, R., Tanaka, T., Togashi, T., Togawa, K., Tokuhisa, A., Tomizawa, H., Tono, K., Wu, S., Yabashi, M., Yamaga, M., Yamashita, A., Yanagida, K., Zhang, C., Shintake, T., Kitamura, H. & Kumagai, N. (2012). Nat. Photon. 6, 540–544. Web of Science CrossRef CAS Google Scholar
Lafferty, J. M. (1951). J. Appl. Phys. 22, 299–309. CrossRef CAS Web of Science Google Scholar
Lu, Z., Yin, S., Zhang, Z., Ren, F. & Lv, X. (2020). Materials, 13, 100. Web of Science CrossRef Google Scholar
Lu, Z., Zhang, Z., Yin, S. & Ren, F. (2018). IEEE International Vacuum Electronics Conference (IVEC), 24–26 April 2018, Monterey, CA, USA, pp. 239–240. IEEE. Google Scholar
Magnuson, M., Butorin, S. M., Guo, J.-H., Agui, A., Nordgren, J., Ogasawara, H., Kotani, A., Takahashi, T. & Kunii, S. (2001). Phys. Rev. B, 63, 075101. Web of Science CrossRef Google Scholar
Mitra, C., Hu, Z., Raychaudhuri, P., Wirth, S., Csiszar, S. I., Hsieh, H. H., Lin, H.-J., Chen, C. T. & Tjeng, L. H. (2003). Phys. Rev. B, 67, 092404. Web of Science CrossRef Google Scholar
Shirasawa, K., Tanaka, T. Seike, A. Hiraya, H. Kitamura (2004). AIP Conf. Proc., 705, 203–206. CrossRef Google Scholar
Tanaka, T., Nishitani, R., Oshima, C., Bannai, E. & Kawai, S. (1980). J. Appl. Phys. 51, 3877–3883. CrossRef CAS Web of Science Google Scholar
Telieps, W. & Bauer, E. (1985). Ultramicroscopy, 17, 57–65. CrossRef CAS Web of Science Google Scholar
Togawa, K., Shintake, T., Inagaki, T., Onoe, K., Tanaka, T., Baba, H. & Matsumoto, H. (2007). Phys. Rev. ST Accel. Beams, 10, 020703. Web of Science CrossRef Google Scholar
Woicik, J. C. (2016). Editors. Hard X-ray Photoelectron Spectroscopy (HAXPES). Springer. Google Scholar
Senba, Y., Ohashi, H., Kishimoto, H., Miura, T., Goto, S., Shin, S., Shintake, T. & Ishikawa, T. (2007). AIP Conf. Proc. 879, 718–721. CrossRef CAS Google Scholar
This article is published by the International Union of Crystallography. Prior permission is not required to reproduce short quotations, tables and figures from this article, provided the original authors and source are cited. For more information, click here.