research papers\(\def\hfill{\hskip 5em}\def\hfil{\hskip 3em}\def\eqno#1{\hfil {#1}}\)

Journal logoJOURNAL OF
SYNCHROTRON
RADIATION
ISSN: 1600-5775

Polished diamond X-ray lenses

crossmark logo

aESRF – The European Synchrotron, 71 Avenue des Martyrs, 38000 Grenoble, France, and bEuclid Techlabs, 365 Remington Blvd, Bolingbrook, IL 60440, USA
*Correspondence e-mail: troth@esrf.fr

Edited by M. Yabashi, RIKEN SPring-8 Center, Japan (Received 23 November 2021; accepted 16 February 2022; online 15 March 2022)

High-quality bi-concave 2D focusing diamond X-ray lenses of apex-radius R = 100 µm produced via laser-ablation and improved via mechanical polishing are presented here. Both for polished and unpolished individual lenses and for stacks of ten lenses, the remaining figure errors determined using X-ray speckle tracking are shown and these results are compared with those of commercial R = 50 µm beryllium lenses that have similar focusing strength and physical aperture. For two stacks of ten diamond lenses (polished and unpolished) and a stack of eleven beryllium lenses, this paper presents measured 2D beam profiles out of focus and wire scans to obtain the beam size in the focal plane. These results are complemented with small-angle X-ray scattering (SAXS) measurements of a polished and an unpolished diamond lens. Again, this is compared with the SAXS of a beryllium lens. The polished X-ray lenses show similar figure errors to commercially available beryllium lenses. While the beam size in the focal plane is comparable to that of the beryllium lenses, the SAXS signal of the polished diamond lenses is considerably lower.

1. Introduction

Diamond is an excellent material for X-ray optics (Shvyd'ko et al., 2017[Shvyd'ko, Y., Blank, V. & Terentyev, S. (2017). MRS Bull. 42, 437-444.]) as it can withstand high heat loads due to its unrivalled thermal conductivity, absorbs little due to its low atomic number (Z = 6), can be obtained in pure and crystalline form with reasonable quality, and, as a refractive element such as a focusing lens, offers a refraction-to-absorption ratio δ/μ (Serebrennikov et al., 2016[Serebrennikov, D., Clementyev, E., Semenov, A. & Snigirev, A. (2016). J. Synchrotron Rad. 23, 1315-1322.]) higher than all typical lens materials except for Be. Since the advent of X-ray focusing lenses (Tomie, 1997[Tomie, T. (1997). X-ray lens. US Patent US5594773A, filed February 1995.]; Snigirev et al., 1996[Snigirev, A., Kohn, V., Snigireva, I. & Lengeler, B. (1996). Nature, 384, 49-51.]), significant effort has been put into the fabrication of diamond X-ray lenses. Due to the difficulty of machining diamond with conventional tools, initial trials deposited CVD diamond into moulds produced in silicon via semiconductor lithography techniques (Snigirev et al., 2002[Snigirev, A. A., Yunkin, V., Snigireva, I., Di Michiel, M., Drakopoulos, M., Kouznetsov, S., Shabel'nikov, L., Grigoriev, M., Ralchenko, V., Sychov, I., Hoffmann, M. & Voges, E. I. (2002). Proc. SPIE, 4783, 1-9.]) or used direct etching of CVD diamond wafers (Nöhammer et al., 2003a[Nöhammer, B., David, C., Rothuizen, H., Hoszowska, J. & Simionovici, A. (2003). Microelectron. Eng. 67-68, 453-460.],b[Nöhammer, B., Hoszowska, J., Freund, A. K. & David, C. (2003b). J. Synchrotron Rad. 10, 168-171.]). These methods led to planar 1D focusing diamond lenses of reduced sagittal aperture (≤110 µm) due to the difficulties in producing deep structures using these planar technologies. Despite later improvements in the processing (Isakovic et al., 2009[Isakovic, A. F., Stein, A., Warren, J. B., Narayanan, S., Sprung, M., Sandy, A. R. & Evans-Lutterodt, K. (2009). J. Synchrotron Rad. 16, 8-13.]; Alianelli et al., 2010[Alianelli, L., Sawhney, K. J. S., Malik, A., Fox, O. J. L., May, P. W., Stevens, R., Loader, I. M. & Wilson, M. C. (2010). J. Appl. Phys. 108, 123107.]), lenses produced by these methods continue to display significant tilt of their side walls, i.e. they are not perpendicular to the wafer surface. Nanofocusing with planar diamond lenses was finally demonstrated (Malik et al., 2013[Malik, A. M., Fox, O. J. L., Alianelli, L., Korsunsky, A. M., Stevens, R., Loader, I. M., Wilson, M. C., Pape, I., Sawhney, K. J. S. & May, P. W. (2013). J. Micromechan. Microeng. 23, 125018.]; Fox et al., 2014[Fox, O. J. L., Alianelli, L., Malik, A. M., Pape, I., May, P. W. & Sawhney, K. J. S. (2014). Opt. Express, 22, 7657-7668.]; Lyubomirskiy et al., 2019[Lyubomirskiy, M., Boye, P., Feldkamp, J. M., Patommel, J., Schoeder, S., Schropp, A., Burghammer, M., Wild, C. & Schroer, C. G. (2019). J. Synchrotron Rad. 26, 1554-1557.]); however, the physical sagittal aperture of these nanofocusing lenses is still below ∼100 µm, and 2D focusing requires stacking of two 1D planar structures with consequent losses in transmission. Thicker 1D focusing structures were obtained by laser cutting of diamond plates (Polikarpov et al., 2016[Polikarpov, M., Polikarpov, V., Snigireva, I. & Snigirev, A. (2016). Phys. Proc. 84, 213-220.]; Kononenko et al., 2016[Kononenko, T. V., Ralchenko, V. G., Ashkinazi, E. E., Polikarpov, M., Ershov, P., Kuznetsov, S., Yunkin, V., Snigireva, I. & Konov, V. I. (2016). Appl. Phys. A, 122, 152.]), with a big challenge being again the verticality of the lens walls, reported to be 1.7° over a cutting depth of 0.6 mm.

More recently, with the emergence of pico- and femto­second pulsed lasers, fabrication of larger structures via laser ablation became viable (Terentyev et al., 2015[Terentyev, S., Blank, V., Polyakov, S., Zholudev, S., Snigirev, A., Polikarpov, M., Kolodziej, T., Qian, J., Zhou, H. & Shvyd'ko, Y. (2015). Appl. Phys. Lett. 107, 111108.], 2017[Terentyev, S., Polikarpov, M., Snigireva, I., Di Michiel, M., Zholudev, S., Yunkin, V., Kuznetsov, S., Blank, V. & Snigirev, A. (2017). J. Synchrotron Rad. 24, 103-109.]; Antipov et al., 2016[Antipov, S., Baryshev, S. V., Butler, J. E., Antipova, O., Liu, Z. & Stoupin, S. (2016). J. Synchrotron Rad. 23, 163-168.]). Ablation allows the fabrication of 1D or 2D focusing lenses into bulk diamond. Since the as-fabricated surface is rough [r.m.s. roughness on the order of 1 µm (Terentyev et al., 2015[Terentyev, S., Blank, V., Polyakov, S., Zholudev, S., Snigirev, A., Polikarpov, M., Kolodziej, T., Qian, J., Zhou, H. & Shvyd'ko, Y. (2015). Appl. Phys. Lett. 107, 111108.]; JJ-X-ray, 2021[JJ-X-ray (2021). Single Crystal Diamond Compound Refractive Lenses, https://www.jjxray.dk/p/xx-single-crystal-diamonds/.])], the focusing properties of these lenses are worse than comparable commercial Be lenses (Lengeler, 2012[Lengeler, B. (2012). Refractive X-ray Lenses: New Developments. Presentation. RWTH Aachen and RXOPTICS, Germany (https://www.rxoptics.de/wp-content/uploads/2018/12/RXOPTICS-Lecture-2012.pdf).]; Lengeler & Lengeler, 2021[Lengeler, B. & Lengeler, D. (2021). RXOPTICS, Germany (https://www.rxoptics.de).]). A post-processing step to improve the surface roughness is thus required. Different methods have been employed: mechanical polishing (Antipov et al., 2018[Antipov, S., Assoufid, L., Grizolli, W., Qian, J. & Shi, X. (2018). Proceedings of the 9th International Particle Accelerator Conference (IPAC'18), 29 April-4 May 2018, Vancouver, BC, Canada, pp. 4057-4058. THPMF011.]) and polishing via wet or dry etches (JJ-X-ray, 2021[JJ-X-ray (2021). Single Crystal Diamond Compound Refractive Lenses, https://www.jjxray.dk/p/xx-single-crystal-diamonds/.]). Polishing using a focused ion beam or excimer laser has also been proposed (Polikarpov et al., 2016[Polikarpov, M., Polikarpov, V., Snigireva, I. & Snigirev, A. (2016). Phys. Proc. 84, 213-220.]). Focused ion beam produced diamond lenses have been shown to produce very smooth lens surfaces and lead to excellent focusing. However, in practice, slow fabrication speeds limit the application of such technologies to the production of few lenses of very small aperture (Medvedskaya et al., 2020[Medvedskaya, P., Lyatun, I., Shevyrtalov, S., Polikarpov, M., Snigireva, I., Yunkin, V. & Snigirev, A. (2020). Opt. Express, 28, 4773-4785.]). Similar sized lenses, used in the visible range and with larger radii, can also be produced via a chemical reflow method (Zhu et al., 2017[Zhu, T.-F., Fu, J., Wang, W., Wen, F., Zhang, J., Bu, R., Ma, M. & Wang, H.-X. (2017). Opt. Express, 25, 1185-1192.]).

We manufactured and characterized bi-concave 2D focusing diamond X-ray lenses produced, as individual elements, via laser ablation and subsequent mechanical polishing. The performance of these lenses is comparable to that of commercial Be lenses, which are regarded as the standard due to their widespread use and continuous development dating back to 2002 (Schroer et al., 2002[Schroer, C. G., Kuhlmann, M., Lengeler, B., Gunzler, T. F., Kurapova, O., Benner, B., Rau, C., Simionovici, A. S., Snigirev, A. A. & Snigireva, I. (2002). Proc. SPIE, 4783, 10-18.]). The lenses were conditioned in [\oslash\,]12 mm frames, which conveniently makes them compatible with existing hardware (e.g. pin-holes, spacers, lens cases, v-blocks and transfocators).

2. Lens fabrication

2.1. Ablation process

Ultrafast (femtosecond) laser ablation of materials has attracted significant interest in recent years due to its promise for high machining accuracy and exceptional quality of the material processing. These appealing properties originate from laser pulse durations which are significantly shorter than the thermal diffusion time at the scale of the beam spot size, thus offering reduced thermal damage and efficient laser pulse utilization (Cheng et al., 2013[Cheng, J., Liu, C., Shang, S., Liu, D., Perrie, W., Dearden, G. & Watkins, K. (2013). Opt. Laser Technol. 46, 88-102.]; Sugioka & Cheng, 2014[Sugioka, K. & Cheng, Y. (2014). Light Sci. Appl. 3, e149.]). Ultrafast laser ablation opened new opportunities for micro-machining materials like diamond which have a limited pool of processing technologies due to their physical properties. The diamond X-ray lenses characterized in this paper are produced by the femtosecond laser micro-machining (Osellame et al., 2012[Osellame, R., Cerullo, G. & Ramponi, R. (2012). Editors. Femto­second Laser Micromachining, Vol. 123 of Topics in Applied Physics. Springer Science & Business Media.]).

Amongst the possible focusing shapes (Sanchez del Rio & Alianelli, 2012[Sanchez del Rio, M. & Alianelli, L. (2012). J. Synchrotron Rad. 19, 366-374.]), 2D-focusing X-ray lenses most commonly assume a bi-concave paraboloid geometry (Lengeler et al., 1999[Lengeler, B., Schroer, C., Tümmler, J., Benner, B., Richwin, M., Snigirev, A., Snigireva, I. & Drakopoulos, M. (1999). J. Synchrotron Rad. 6, 1153-1167.]). When producing such a shape via laser ablation, we decompose this profile into circular layers with diameters that decrease parabolically with depth. In order to remove a circular layer, the laser beam is steered by motorized mirrors covering a circular area uniformly. To achieve the required accuracy of the shape a large set of parameters has to be optimized: the beam focus size and convergence as well as the laser flux and pulse duration. We utilize a green 515 nm laser with a 200 fs pulse duration and average power of few hundred milliwatts depending on the focusing configuration. The unavoidable motion errors, triggering jitter and re-deposition of the ablated material result in figure errors, that is, deviations of the resultant profile from the design geometry. The lack of in situ metrology makes it virtually impossible to iteratively eliminate correlated errors by adjusting the ablation recipe.

2.2. Raw material

The two main techniques for producing synthetic diamonds are high-pressure high-temperature (HPHT) growth and chemical vapour deposition (CVD). HPHT diamonds present a better crystalline structure; however, CVD diamonds can be produced in larger sizes and are less expensive (Shvyd'ko et al., 2017[Shvyd'ko, Y., Blank, V. & Terentyev, S. (2017). MRS Bull. 42, 437-444.]). Both types of synthetic diamond come in various grades, which differ in growth parameters and in spurious nitrogen content. The lenses used in this study were structured in low dislocation density HPHT (100)-oriented diamond plates.

Fig. 1[link] compares the white-beam topography for an HPHT and a CVD diamond. Due to lower dislocation densities in HPHT diamond compared with CVD diamond, Fig. 1[link](a) is more homogeneous than Fig. 1[link](b). For the purposes of laser-cutting, we have not observed any substantial difference using several grades of diamonds, i.e. polycrystalline and single-crystalline CVD and HPHT with different nitrogen concentration. The femtosecond-laser cutting process does not significantly increase the dislocation density around the lens structures as shown in Fig. 1[link](c). We have observed, however, a difference in the polishing process removal rate and uniformity depending on the diamond grade.

[Figure 1]
Figure 1
X-ray white beam topography images. (a) HPHT diamond, (b) single-crystal CVD diamond and (c) CVD diamond plate with lenses cut in it. Diamonds in this image are 3 mm × 3 mm × 0.5 mm in size.

In terms of X-ray transport and beam focusing, one expects that a diamond with a higher degree of crystallinity will produce less small-angle X-ray scattering (SAXS). However more important to the performance of a diamond lens are its figure error and surface roughness. The choice of diamond grade has a significant impact on the total cost of the lens and, if a lower grade diamond is acceptable for certain applications, the cost of the diamond lenses can be reduced. Now that the quality of diamond lenses presented here is substantially improved, it is possible and desirable to perform a dedicated study on the influence of the raw material for future diamond lens production.

2.3. Post-polishing

Depending on ablation parameters, the as-cut surface roughness of the diamond lens is 300–500 nm Sa (ISO 25178, which defines a surface extension of Ra, arithmetical mean deviation of heights from the assessed profile – ISO 4287), obtained by confocal microscopy at 50× magnification. To reduce these values we developed a post-ablation chemical–mechanical polishing procedure for the diamond lenses. In this process, a conformal needle (polishing bit) is lowered into the diamond lens along with 0.1 µm diamond slurry and spun inside for several hours.

Fig. 2[link] shows the basic setup and typical polishing results. A high-speed, high-accuracy spindle is used to spin the polishing bit inside the lens. Note that, due to the small size of the lens and the polishing bit, a microscope is used to align the polishing bit with the lens. The polishing process is a hybrid of chemical etching and free abrasive polishing. Multiple parameters must be optimized: polishing bit material, slurry solvent and grit size, contact pressure, and rotational speed. Since the surface of the lens is curved (Fig. 2[link], middle), there is an uneven force perpendicular to the surface when a downward pressure is applied. This leads to uneven removal of material. To compensate this effect we introduce periodic pressure applied sideways. The polishing process has been fine-tuned and is able to maintain a quasi-uniform removal rate along the complete surface of the lens. The lens surface is polished to optical transparency with local micro-roughness of about 20 nm Sa. The final result is presented in Fig. 3[link], which was captured through the polished and transparent side wall of the diamond plates.

[Figure 2]
Figure 2
Photograph and sketch of the polishing process (left and middle). On the right, an SEM image shows the diamond lens surface at an interface between a polished and intentionally unpolished region.
[Figure 3]
Figure 3
Microscope images of an unpolished (left) and a polished (right) lens. The images are taken through the polished side wall of the diamond plate. Both lenses have a physical aperture of Aphys ≃ 440 µm.

2.4. Packaging

In general, X-ray lenses are stacked together to obtain short focal lengths. These compound refractive lenses (CRLs), as those stacks are called, can be composed of several dozen individual lenses. An important factor to be considered for adopting CRLs in synchrotron beamlines is how well the lenses can be aligned with respect to each other as misalignments between the elements of a CRL will degrade the lens performance (Andrejczuk et al., 2010[Andrejczuk, A., Krzywiński, J., Sakurai, Y. & Itou, M. (2010). J. Synchrotron Rad. 17, 616-623.]; Celestre et al., 2020b[Celestre, R., Chubar, O., Roth, T., Sanchez del Rio, M. & Barrett, R. (2020b). Proc. SPIE, 11493, 114930J.]). A common solution applied to individually produced 2D X-ray lenses is to house them in 12 mm-diameter precision-machined disks, where the lenses should be centred within 1 µm or 2 µm. This is the case, for example, with commercial Be, Al and Ni embossed lenses.

We fabricate our support disks from copper alloy (bronze) with diameters within a 2–3 µm tolerance. Prior to laser ablation, the diamond plate in the form of a truncated cone is pressed carefully into the disk to avoid any tilt. Once the diamond is properly set, the lens profile can be micromachined in the centre of the disk. To ensure that both the back- and front-paraboloidal sections overlap, we mount the lens in a small stationary v-block shown in Fig. 4[link](a). We also use fiducial markings on the coin to align them to the v-block to determine the lens orientation during ablation, see Fig. 4[link](b). By packing our diamond lens in the same form factor as the industry-standard they can be readily integrated in beamlines using existing hardware (e.g. pin-holes, spacers, lens cases, v-blocks and transfocators) coexisting harmoniously with already acquired lenses. Fig. 4[link](c) shows lens stacks in a commercial lens holder.

[Figure 4]
Figure 4
Packaging of diamond lens: (a) mini v-block for lens ablation, (b) lens support disk containing a diamond with an ablated lens in the middle and fiducial markings indicating azimuthal orientation during the ablation process, (c) lens stacking for an experiment in a commercial lens holder. Lenses are housed in 12 mm-diameter bronze disks.

2.5. Visible-light metrology

Despite not being implemented as an in situ measurement, we use scanning confocal laser microscopy for fine-tuning the ablation and post-polishing processes. This preliminary inspection tool is able to quickly provide information regarding the geometric aperture, refracting surface penetration depth, parabolic shape and radius of curvature of individual refracting surfaces as shown in Fig. 5[link](a).

[Figure 5]
Figure 5
Laser scanning confocal microscopy of an unpolished diamond lens: (top) 3D reconstruction of front refractive surface, (bottom) residual profile after extraction of a paraboloid fit.

Removing the best paraboloid fit from the metrology data, we are able to determine the figure errors as displayed in Figs. 5[link](b) and 5[link](c), showing we achieve sub-micrometre r.m.s. figure errors for the laser-machined paraboloid. One of the limitations of this technique is the accurate determination of the mutual alignment of the measurements from the front and back surfaces in a bi-concave lens. Also, though measuring as-ablated surfaces is relative straightforward due to the elevated roughness and light scattering, polished lenses with their smooth surfaces and transparency are very difficult to measure using visible light confocal microscopy. A workaround to this inconvenience is applying a very thin conformal coating to reduce the transparency to visible light and make the laser scanning measurement possible.

3. Lenses and lens stacks measured in this work

In this paper, we show experimental results obtained using individual lenses of three different types as well as results of three different lens stacks. The three types of individual lenses are (i) unpolished R = 100 µm diamond lenses; (ii) polished R = 100 µm diamond lenses; and (iii) commercial R = 50 µm Be lenses produced by RXOptics (Lengeler & Lengeler, 2021[Lengeler, B. & Lengeler, D. (2021). RXOPTICS, Germany (https://www.rxoptics.de).]), where R represents the apex radius of curvature of the sagittal and meridional parabolic sections. The three different lens stacks are: (A) a stack of N = 10 of the unpolished R = 100 µm diamond lenses, (B) a stack of N = 10 of the polished R = 100 µm diamond lenses, and (C) a stack of N = 11 of the commercial R = 50 µm Be lenses. The diamond lenses have a crystal thickness LC* of roughly 500 µm (the lens thickness varied between 471 µm and 515 µm) and a distance between the apices of the paraboloidal sections (t or web thickness) of about ∼20 µm. The Be lenses are pressed into LBe = 1 mm-thick Be discs and have an apex width of about 30 µm.

Comparing R = 100 µm diamond lenses with R = 50 µm Be lenses is reasonable: first, the focusing strength of a single lens can be characterized by its focal length f = R/(2δN) with N = 1 for a single lens, R the lens radius and δ the refractive index decrement of the element used. At photon energies between 5 keV and 50 keV, the ratio δC*/δBe varies slightly around 2.14, see Appendix A[link]. This makes an R = 100 µm diamond lens about equivalent to an R = 50 µm Be lens. Secondly, as the physical aperture of a lens is given as Aphys = 2[(Lt)R]1/2, and in our case we have LBeRBeLC*RC*, we obtain also very similar physical apertures of Aphys ≃ 440 µm.

Our two diamond lens stacks contain N = 10 individual lenses (unpolished or polished). We can fine-tune the number NBe of Be lenses to get the best equivalent Be lens stack as follows,

[N_{\rm Be} = N_{\rm C^{\,*}}{{\delta_{\rm C^{\,*}}} \over {\delta_{\rm Be }}}{{R_{\rm Be}} \over {R_{\rm C^{\,*}}}}\simeq 10.7. \eqno(1)]

We thus use N = 11 lenses for the Be lens stack.

4. At-wavelength metrology via X-ray speckle tracking

Although helpful in order to study surface roughness and measure the depth and aperture of the machined lens, the initial inspection using visible-light metrology after lens production suffers from limitations: it only probes one side of a bi-concave lens at a time and is insensitive to sub-surface defects; it also does not measure the alignment and mutual tilt of the front- and back-focusing surfaces. For the polished lenses, little signal returns from the steeper parts of the parabolic surfaces. To overcome those drawbacks and recover figure errors in projection approximation, we use X-ray (near-field) speckle vector tracking (XSVT) (Berujon et al., 2020b[Berujon, S., Cojocaru, R., Piault, P., Celestre, R., Roth, T., Barrett, R. & Ziegler, E. (2020b). J. Synchrotron Rad. 27, 284-292.]) which is an at-wavelength metrology technique.

In the differential metrology mode of XSVT, the experiment consists of a monochromatic beam with sufficient lateral coherence illuminating a random static modulator and projecting the speckle pattern generated by it onto a 2D imaging detector. A reference dataset is taken by transversely shifting the random modulator across the beam and registering N images. A lens (-stack) is then introduced in the beam downstream of the speckle-modulator at a distance d from the detector. A second dataset is taken by once again scanning the random modulator across the beam and registering N images at the exact positions where the reference dataset was taken. By comparing both datasets, the lateral displacement map νx(x, y), νy(x, y) of the speckle pattern at the detector plane is calculated. With the knowledge of the distance d, the deflection angle (αx, αy) ≃ (νx, νy)/d is retrieved. This deflection angle is related to the beam phase gradient ∇ϕ by the wavenumber k. By numerical integration of the phase gradients obtained experimentally, the beam phase ϕ(x, y) can be calculated. The projected thickness of the probe is calculated as Δz(x, y) = −ϕ(x, y)/kδ. The figure errors in the projection approximation are recovered by removing a paraboloid of revolution (2D focusing). The XSVT technique is described in more detail in Section 2.2.3 in the work by Berujon et al. (2020b[Berujon, S., Cojocaru, R., Piault, P., Celestre, R., Roth, T., Barrett, R. & Ziegler, E. (2020b). J. Synchrotron Rad. 27, 284-292.]) and Section 3.1.1 in the work by Berujon et al. (2020a[Berujon, S., Cojocaru, R., Piault, P., Celestre, R., Roth, T., Barrett, R. & Ziegler, E. (2020a). J. Synchrotron Rad. 27, 293-304.]).

Our XSVT experiments were performed at the ESRF-EBS beamline BM05 (Ziegler, 2004[Ziegler, E. (2004). AIP Conf. Proc. 705, 436-439.]) using a monochromatic beam, Si(111) double-crystal monochromator, at 17 keV for single-lens metrology (Section 4.1[link]) and 30 keV for lens stack measurements (Section 4.2[link]). The change in energy for the stack measurement is to keep d sufficiently large to avoid the speckle grains collapsing into each other, causing the tracking algorithm to fail. The measurements at lower energies used stacked cellulose acetate membrane filters with a pore size of ∼1.2 µm as the speckle generator, whereas the measurements at 30 keV used stacked sheets of 1200 grit silicon carbide abrasive paper. The random modulators were mounted on piezoelectric nano-positioners to ensure high position repeatability between both datasets. The distance d between probe and detector was kept at 800 mm for the 17 keV measurements and 500 mm for the stacked lenses metrology. The detector was a pco.edge sCMOS sensor coupled to a 10× microscope objective imaging a ∼17 µm-thick GGG:Eu scintillator. The effective pixel size is 0.635 µm. The lateral resolution has been evaluated at 17 keV only, where it is better than 1.5 µm.

This section presents the XSVT results of unpolished and polished X-ray lenses and compares their shape errors to those of the equivalent R = 50 µm Be lenses of similar geometric aperture. A selection of these lenses can then be used to form three stacks of similar focusing strength that are also measured and presented: 10 × unpolished, 10 × polished diamond and 11 × Be lenses.

4.1. Individual lens measurements

The metrology of individual lenses allows quantification of the figure errors of the lenses after the laser ablation machining process and can help to fine-tune this process. Furthermore, it can investigate the effect of post-polishing on the figure errors of the X-ray lenses.

Fig. 6[link] shows representative examples of lens radiographs and figure errors for the three lens types used in this work. The presence of concentric circle-like- and bent-radial structures in the unpolished diamond lens radiography is evident – these features are also present in the accumulated figure errors for the same lens [cf. Figs. 6[link](a) and 6[link](b)]. These features originate from the rough surface after the ablation process and are completely removed by polishing as shown in Figs. 6[link](c) and 6[link](d). The post-polishing, however, introduces rotational symmetric figure errors to the lens, without significant change to the figure error r.m.s. value (σ) over the useful aperture.

[Figure 6]
Figure 6
Single-lens radiograph and figure error for each investigated lens type: unpolished R = 100 µm C* lens (top,), polished C* lens (middle) and R = 50 µm Be lens (bottom). Radiographs were taken 800 mm downstream of the sample, enhancing edge effects in phase-contrast imaging (dark rings delimiting the lens geometric aperture).

The Be lens radiograph is very homogeneous. The r.m.s. figure error of the Be lens is of a similar size to that of both diamond lenses. However, the figure errors of the Be lens can be well described by only lower-order Zernike polynomials, i.e. they have a smoother long-range order, plus a high-frequency short-range noise, possibly due to the Be microstructure.

The observations based on Fig. 6[link] are representative of all measured unpolished and polished diamond and Be lenses. Fig. 7[link] summarizes some key parameters (lens radius, aperture, r.m.s. figure error and optical path difference) for 14 unpolished and 25 polished diamond lenses comparing them against the metrology of 24 equivalent Be lenses. We can see that polishing the diamond lenses has the effect of slightly increasing the radius of curvature R. The unpolished lenses have a mean radius of curvature of R = 95.4 ± 0.6 µm, whereas for the post-processed lenses R = 97 ± 1 µm, Fig. 7[link](a). As a reference, for the Be lenses R = 48.7 ± 0.3 µm [cf. Fig. 7[link](b)]. The target radii are 100 µm for C* and 50 µm for Be lenses.

[Figure 7]
Figure 7
Dispersion plots of the lenses main figures of merit obtained with XSVT metrology of individual lenses. The OPD is calculated for E = 10 keV.

The geometric aperture of the diamond lenses is systematically smaller than those of the equivalent Be lenses as shown in Fig. 7[link](c). The probable reasons for this difference are threefold: (i) mismatch between the designed and executed penetration depth of the parabolic section (refracting surface), resulting in an increased distance between parabolic surfaces (t); (ii) difference between real and expected diamond thickness L; (iii) the radius of curvature R of the lens. Mismatch between the penetration depths and misalignment between front and back refracting surfaces of the Be lenses explain the lower tail in Fig. 7[link](c). These fabrication issues also occur in the production of the diamond lenses but are currently less recurrent. Another factor that contributes to the apparent reduction in the geometric aperture is that diamond gives stronger edge contrast in phase-contrast imaging when compared with beryllium at the same energy – this is manifested as dark ring delimiting the lens area in the radiographs from Fig. 6[link]. While this has no effect on the geometric aperture, it reduces the area from which metrology data can be extracted and, as a consequence, the calculated useful aperture plotted in Fig. 7[link](c) is underestimated.

Lastly, the figure errors of the diamond lenses (unpolished and polished) are slightly lower than those of commercial Be lenses: σ = 0.85 ± 0.09 µm, σ = 0.9 ± 0.2 µm and σ = 1.1 ± 0.1 (5) µm, respectively. Although the mechanical polishing does slightly increase the nominal figure error and more significantly its dispersion, they are still close to the values measured on the commercial Be lenses [cf. Fig. 7[link](d)]. Note that, although the r.m.s. value of the figure errors is not significantly altered by the polishing, the spatial distribution is (see Fig. 6[link]). From the figure errors it is possible to obtain the optical path length (OPD), which expresses the material-dependent phase shift as OPD = kδσ. This dimensionless figure of merit, shown in Fig. 7[link](e), is energy dependent. However, the ratio δC*/δBe stays around ∼2.14 for a wide range of energies and the general trend in Fig. 7[link](e) is retained: despite having slightly higher figure errors, at a fixed energy Be lenses have a lower associated OPD than both unpolished and polished diamond lenses.

4.2. Measurements of lens stacks

X-ray lenses are generally used as CRL stacks. The metrology of stacked lenses is important because it (i) allows simulation of the performance of the lens stack (Celestre et al., 2020a[Celestre, R., Berujon, S., Roth, T., Sanchez del Rio, M. & Barrett, R. (2020a). J. Synchrotron Rad. 27, 305-318.]) and (ii) permits the development of strategies for the mitigation of aberrations, see Section 4.3[link]. The measurements of 10 × unpolished, 10 × polished diamond and 11 × Be lens stacks are shown in Figs. 8[link] and 9[link].

[Figure 8]
Figure 8
Lens-stack metrology using XSVT. Top: 10 × unpolished diamond lenses, middle: 10 × polished diamond lenses, bottom: 11 × Be lenses. The coefficients of the polynomial decomposition in (e) are shown in Fig. 9[link].
[Figure 9]
Figure 9
Zernike circle polynomial decomposition of the error profiles in Fig. 8[link]. The terms Z1 to Z4 are suppressed as they account for piston, x and y tilts, and defocus, respectively, and are not strictly optical aberrations. The terms Z5 and Z6 represent astigmatism, Z7 and Z8 show coma, and Z9 and Z10 show tetrafoil aberrations. Z11 stands for spherical aberration. Z12 onward are higher-order variations of the aberration terms from Z5 and Z11. The orange bars are rotationally symmetric indicating primary to tertiary spherical aberrations.

The characteristic laser machining marks on the rough surface of the unpolished diamond lenses, i.e. circle-like- and bent-radial structures, are still present when the lenses are stacked, see Figs. 8[link] [top row (a) and (d)]. For this particular set of lenses, the asymmetric figure errors tend to reinforce due to unfavourable azimuthal lens alignment inside the lens cassette [Fig. 9[link] (top row)] which can be mitigated by rotating the lenses individually around the optical axis (Osterhoff et al., 2017[Osterhoff, M., Detlefs, C. & Ferrero, C. (2017). Proc. SPIE, 10388, 103880L.]).

The polished diamond lens stack shows a more homogeneous radiograph and a complete change in the topography of the error distribution – compared with the unpolished stack – which displays stronger rotational symmetry [Fig. 8[link] (middle row (d) and orange bars in Fig. 9[link] (middle row)]. The change in error distribution, which is already visible in the metrology of the individual lenses, is expected from the post-polishing process presented in Section 2.3[link].

The spherical aberrations of the diamond lenses, here accentuated by post-polishing, are also commonly found in commercial Be lenses as presented in Figs. 8[link] and 9[link] (bottom row) and extensively reported (Celestre et al., 2020a[Celestre, R., Berujon, S., Roth, T., Sanchez del Rio, M. & Barrett, R. (2020a). J. Synchrotron Rad. 27, 305-318.]; Dhamgaye et al., 2020[Dhamgaye, V., Laundy, D., Baldock, S., Moxham, T. & Sawhney, K. (2020). J. Synchrotron Rad. 27, 1518-1527.]; Seiboth et al., 2020[Seiboth, F., Brückner, D., Kahnt, M., Lyubomirskiy, M., Wittwer, F., Dzhigaev, D., Ullsperger, T., Nolte, S., Koch, F., David, C., Garrevoet, J., Falkenberg, G. & Schroer, C. G. (2020). J. Synchrotron Rad. 27, 1121-1130.]). The reason here is not a polishing process but imperfections in the plastic-forming process used for the lens manufacture or in the manufacturing of the paraboloidal punches on a lathe. A more quantitative analysis of the accumulated figure errors shows that the polished lens stack has r.m.s. figure errors of σ = 4.36 µm over the entire useful aperture against σ = 5.60 µm of the Be lens stack. Although in terms of figure errors polished diamond lens stacks compare favourably with Be stacks, the optical path difference still compares unfavourably for diamond lenses due to their higher index of refraction: OPDC*CRL = 0.56 against OPDBeCRL = 0.33 at 10 keV for example. The dependence of the r.m.s. figure errors on the lens half aperture is shown in Fig. 8[link](b) for all three stacks.

4.3. Possible correction of figure errors

The accumulated profile error of the polished lens stack shown in Fig. 8[link] [middle row (d)] has strong rotational symmetry, as shown by the amplitude of the orange bars (primary to tertiary spherical aberration) in Fig. 9[link] (middle). This is particularly amenable to reduction of the wavefront aberrations via the use of azimuthally symmetric refractive phase plates (Seiboth et al., 2020[Seiboth, F., Brückner, D., Kahnt, M., Lyubomirskiy, M., Wittwer, F., Dzhigaev, D., Ullsperger, T., Nolte, S., Koch, F., David, C., Garrevoet, J., Falkenberg, G. & Schroer, C. G. (2020). J. Synchrotron Rad. 27, 1121-1130.]; Dhamgaye et al., 2020[Dhamgaye, V., Laundy, D., Baldock, S., Moxham, T. & Sawhney, K. (2020). J. Synchrotron Rad. 27, 1518-1527.]). Fig. 10[link] shows the approximately 50% reduction of the effective figure errors of the polished diamond lens stack which should be achievable by the implementation of an ideal azimuthally symmetric diamond phase-corrector calculated to minimize the spherical aberrations.

[Figure 10]
Figure 10
(a) Measured figure errors of the 10 × polished diamond lens stack. (b) Closest calculated azimuthally symmetric figure error approximation of (a). A phase corrector of inverted thickness variation profile is required to reduce the wavefront aberrations. (c) Calculated residual effective figure errors expected from the combination of the lens stack and phase corrector.

5. Beam caustics and 2D intensity profile cuts along the beam path

Metrology of single-lens elements and lens stacks is important; however, on a synchrotron beamline, the aim of using focusing lenses is usually to achieve a small focused probe with minimal scattering, halo or side lobes. Using a 2D detector with high spatial resolution, we recorded the transverse X-ray beam profile in the vicinity of the focal plane, when using each of the lens stacks A, B and C.

The experiment was performed on ID06 (Kutsal et al., 2019[Kutsal, M., Bernard, P., Berruyer, G., Cook, P. K., Hino, R., Jakobsen, A. C., Ludwig, W., Ormstrup, J., Roth, T., Simons, H., Smets, K., Sierra, J. X., Wade, J., Wattecamps, P., Yildirim, C., Poulsen, H. F. & Detlefs, C. (2019). Mater. Sci. Eng. 580, 012007.]) using a 10 keV beam after a Si(111) double-crystal monochromator. Each stack was mounted on a motorized hexapod alignment stage positioned 54 m from the X-ray source point (λu = 27 mm permanent magnet undulator), with identical experimental conditions (slit settings, vacuum pipes and in-air sections, etc.). A 2D CCD detector (Atmel TH7899M, 14 µm × 14 µm pixel size) captured the visible light generated by a 25 µm-thick LuAG:Ce scintillator via a 10× objective lens, a 0.9× extension tube and a 2.5× eye piece. The effective pixel size was 0.62 µm (Kutsal et al., 2019[Kutsal, M., Bernard, P., Berruyer, G., Cook, P. K., Hino, R., Jakobsen, A. C., Ludwig, W., Ormstrup, J., Roth, T., Simons, H., Smets, K., Sierra, J. X., Wade, J., Wattecamps, P., Yildirim, C., Poulsen, H. F. & Detlefs, C. (2019). Mater. Sci. Eng. 580, 012007.]). The distance between the lens stack and the detector scintillator could be varied. At 10 keV, the expected focal lengths of the lens stacks are given in Table 1[link].

Table 1
Characteristics of the lens stacks at 10 keV and the consequent focusing parameters

f is the calculated focal length of the stack, p is the distance between the lens stack and the photon source, and q is the image distance calculated from f and p via the thin-lens equation. M is the magnification when imaging the source, L is the thickness of the lens material at the lens rim, Dphys is the physical aperture and Deff is the effective aperture reduced by X-ray absorption in the thicker lens regions [see equation (27) of Kohn (2017[Kohn, V. G. (2017). J. Synchrotron Rad. 24, 609-614.])] for 10 keV.

  N R (µm) f (mm) p (m) q (mm) M L (mm) Dphys (µm) Deff (µm)
C* 10 100 685 54 694 78 0.5 436 231
Be 11 50 666 54 674 80 1 442 361

Fig. 11[link] shows the beam size full width at half-maximum (FWHM) as measured by the CCD camera and fitted with a 2D Gaussian while the detector is scanned along the X-ray beam path. All three lens stacks have a focal plane in the vicinity of 670 mm and show similar minimum beam size, which is close to the optimal resolution of the CCD camera.

[Figure 11]
Figure 11
Beam caustics and profiles at the focal plane.

Fig. 12[link] presents images of the X-ray beam intensity distribution at fixed distances from the focal position, namely 25 mm upstream of the focus, at the focus, 25 mm downstream and 50 mm downstream of the focal position.

[Figure 12]
Figure 12
X-ray beam intensity profile as measured 25 mm upstream of focus, at focus, and 25 mm and 50 mm after the focus. Top row: 10 × unpolished diamond lenses. Middle row: 10 × polished diamond lenses. Bottom row: 11 × beryllium lenses. Note that the colour range is different for each column and has been plotted using a power law with exponent 0.33 (gamma correction) in order to highlight less-intense regions.

The beam sizes (both vertical and horizontal) for the Be lens stack increase faster when getting further from the focal plane, compared with both diamond lens stacks. The origin for this behaviour is the larger effective aperture of the Be lens stack (see Table 1[link]), which implies that more photons farther off the optical axis are transmitted by the Be lenses compared with the diamond lenses. At low photon energies, 10 keV for example, Be lenses are the more efficient focusing element, but this advantage is greatly reduced at higher X-ray energies. Here, at 10 keV and with an incoming X-ray beam size upstream of the lenses of approximately 1 mm × 1 mm that is slit down to 450 µm × 450 µm, the measured integrated detector signal after the Be lenses is about 1.8× higher than in the case of the diamond lens stack. This is in agreement with a calculated transmission of a flat-square beam 450 µm × 450 µm in size through a lens with a physical lens aperture of 440 µm and a web thickness tmin of 30 µm as a function of the projected thickness Δ(x, y), that is [T \propto \smallint\exp[-\mu\Delta(x,y)]\,{\rm d}x\,{\rm d}y]. For the beryllium and both diamond lenses: [T^{\,\rm on \ apert.}_{\rm 11\,Be}=0.791] and [T^{\,\rm on \ apert.}_{\rm 10\,C*}= 0.463], giving a ratio of 1.71. As an example for higher energies, at 30 keV, while maintaining the focal length using nine times as many lenses (NBe = 99, NC* = 90), the advantage in transmission of the Be stack is reduced to 1.27 via a similar calculation.

6. Wire scan measurements: beam size at focus

In order to overcome the lateral resolution limit of the 2D CCD camera system, we installed a 200 µm-diameter tungsten wire on precision yz translation stages (Newport MFA-PP), followed by a large surface area Si p-i-n diode connected to a pico-ampere meter. The tungsten wire was scanned both vertically and horizontally through the beam (step size of 0.25 µm), and this experiment was repeated with a slightly varying lens-to-wire distance. The measured intensity profile with the diode shows an S-shaped curve between a position outside the beam and when blocking the beam. After a Gaussian fit of the numerically differentiated signal, we calculate the projected FWHM beam size in the horizontal and in the vertical directions.

Fig. 13[link] shows the measured FWHM beam size along both the vertical (dark colours, filled symbols) and the horizontal (bright colours, open symbols) direction for the three lens stacks as a function of the centre-of-lens-stack to wire distance. This figure is consistent with Fig. 11[link]; however, the resulting FWHM are slightly lower, as the result is not broadened by the detector lateral resolution.

[Figure 13]
Figure 13
Beam sizes in the vicinity of the focal plane as measured by scanning a [\oslash\,]200 µm tungsten wire through the X-ray beam.

As can be seen from the position of the focal plane in Fig. 13[link], the radii of the polished lenses are about 1.6% larger than the radii of those unpolished. Polishing removes material and thus tends to increase the lens radius. This is in agreement with the at-wavelength metrology results, see Fig. 7[link](a). For the central position for each of the lenses in Fig. 13[link], the corresponding raw data of the wire scan, its derivative (arbitrary units, not shown) and a Gaussian fit to this derivative are shown in Fig. 14[link].

[Figure 14]
Figure 14
Smallest measured beam size using the wire scan technique for all three lens stacks (top: unpolished C* lenses, middle polished C* lenses, bottom Be lenses). We first take the numerical derivative ΔIdiode/Δx of the beam intensity measured via the current generated in a p-i-n photodiode (raw signal: coloured lines with points). This derivative (black dots) is fitted by a Gauss function (solid lines). Left column: horizontal beam size; right column: vertical beam size.

The measured beam sizes are larger than expected. At an ESRF beamline, after the EBS upgrade, the FWHM X-ray source size in the 16 bunch filling mode is 70 µm × 18 µm (horizontal × vertical). In geometric optics, using M ≃ 79 from Table 1[link], this would give a focused beam size of approximately 0.88 µm × 0.23 µm. Considering Gaussian optics and the diffraction limit corresponding to the effective aperture of each lens stack, as well as slightly different focal lengths, that changes the expected FWHM beam size in the focal plane to 0.883 µm × 0.255 µm for Be and 0.924 µm × 0.314 µm for diamond, where we followed equation (44) from the work by Lengeler et al. (1999[Lengeler, B., Schroer, C., Tümmler, J., Benner, B., Richwin, M., Snigirev, A., Snigireva, I. & Drakopoulos, M. (1999). J. Synchrotron Rad. 6, 1153-1167.]). The vertical values are diffraction-limited and differ significantly for the two materials as a consequence of the different effective apertures (see Table 1[link]). A point source would be imaged to a 0.10 µm image for the case of the Be lens stack, and a 0.20 µm image for the diamond lens stack. Our measurements for the polished diamond lens stack are larger by a factor 1.7 in the horizontal and a factor 3 in the vertical. For the Be lens stack, these factors are 1.6 (horizontal) and 3.7 (vertical).

The above calculations consider ideal lens shapes, however. As we measured larger values, these deviations can come from lens shape errors, lens surface roughness effects (as seen in the larger focal sizes of the unpolished lenses) and also possibly vibrational beam size broadening by a vertically deflecting, cryogenically cooled double-crystal monochromator as present on ID06. The effect of the lens shape errors can be evaluated via simulations, as we have measured the error profiles for all lens stacks.

7. Simulations of the 2D profile cuts along the beam path and beam size at focus

We used the metrology profiles obtained with XSVT in Section 4.2[link] [see Fig. 8[link](d)] to simulate the X-ray beam focusing by the lens stacks used in this work. These partially coherent simulations were performed using the SRW macro-electrons method (Chubar & Elleaume, 1998[Chubar, O. & Elleaume, P. (1998). Proceedings of the 6th European Particle Accelerator Conference (EPAC'98), 22-26 June 1998, Stockholm, Sweden, pp. 1177-1179. THP01G.]; Chubar et al., 2011[Chubar, O., Berman, L., Chu, Y. S., Fluerasu, A., Hulbert, S., Idir, M., Kaznatcheev, K., Shapiro, D., Shen, Q. & Baltser, J. (2011). Proc. SPIE, 8141, 814107.]) and the refractive optics Python library described by Celestre et al. (2020b[Celestre, R., Chubar, O., Roth, T., Sanchez del Rio, M. & Barrett, R. (2020b). Proc. SPIE, 11493, 114930J.]), which implements the modelling of phase imperfections in refractive optics presented by Celestre et al. (2020a[Celestre, R., Berujon, S., Roth, T., Sanchez del Rio, M. & Barrett, R. (2020a). J. Synchrotron Rad. 27, 305-318.]). The calculations here replicate the ID06 beamline under similar conditions to the experiments described in Sections 5[link] and 6[link].

The first row of Fig. 15[link] shows the simulated focusing of the unpolished lens stack with strong similarity to the experimental data shown in the top row of Fig. 12[link]. Features like the central lobe 25 mm upstream of the focal plane and the ring profile downstream are very well reproduced – see for example the concentric quarter of ring formation (in orange/yellow) at +50 mm in both the experimental and and the simulated data. The tilted oval shapes at −25 mm and +25 mm and the orientation of the major axes are also reproduced. The simulations in Fig. 15[link] (middle row) also reproduce important features from the polished stack, namely the concentric ring-like structures observed up and downstream of the focal plane. The central lobe seen at +50 mm is also visible in the simulations, along with a few concentric rings, also visible in Fig. 12[link]. The beam focusing by the Be lens stack shown in Fig. 15[link] (bottom row) is also in good agreement with the experimental data in Fig. 12[link] (e.g. with a central lobe observed upstream of the focal plane and ring structures downstream). The simulations also describe well the beam scattering around the focal spot (0 mm) and the fact that the beam sizes at +50 mm are different. Note that the simulations have a far higher lateral resolution than the experimental data and do not suffer from any degradation (e.g. vibrations, beam instabilities, detector noise etc.), hence the beam features are better defined and richer in detail than the experimental data.

[Figure 15]
Figure 15
Simulated X-ray beam profile simulated 25 mm upstream of focus, at the image plane, and 25 mm and 50 mm after the focal plane. Top row: 10 × unpolished diamond lenses. Middle row: 10 × polished diamond lenses. Bottom row: 11 × Be lenses. Note the different intensity range for each column. The plots use a gamma correction (γ = 0.33) in order to highlight weaker intensity regions.

The high resolution of the simulations can be used to evaluate the beam size around the focal plane. By projecting the intensity horizontally and vertically and performing a Gaussian fit of the resulting profiles, we obtain results that can be compared with the measurements in Section 6[link]. The simulated beam focusing can be seen in Fig. 16[link], which agrees qualitatively with Fig. 13[link]. The introduction of figure errors to the simulations show clear degradation of the focal spot size, which is more evident for the unpolished diamond lens stack. For reference, ideal focusing is presented in Figs. 16[link](d) and 16[link](e). In general, we see a worse performance for the unpolished C* stack and very similar performances for the polished C* and Be stacks, with the latter being slightly better. The steeper caustic from the Be stack (related to larger effective aperture and shorter focal length) is also shown by the simulations. Regarding experimental data (Fig. 14[link]), simulations are more optimistic in terms of beam sizes at the focal plane. These discrepancies, stronger for the vertical plane, might be partially explained by vibrations in the monochromator or thermal deformations of the first crystal of the monochromator. A compilation of the beam sizes for the different stacks is presented in Table 2[link].

Table 2
Summary of beam sizes in micrometres obtained from simulations (Sim.) and experimental (Exp.) data for different lens stacks

  Diamond Be
    Unpolished Polished      
Stacks Ideal Sim. Exp. Sim. Exp. Ideal Sim. Exp.
Horizontal 0.94 1.50 2.05 1.08 1.61 0.93 1.04 1.55
Verical 0.26 0.92 1.49 0.38 0.98 0.23 0.30 0.98
[Figure 16]
Figure 16
Simulated beam sizes (FWHM) in the vicinity of the focal plane for different lens stacks. Horizontal values are represented by lines with black circle markers and the vertical profile sizes by lines with crosses.

8. Small-angle X-ray scattering

The absorption of X-rays in a stack of lenses is an important characteristic of the lens for X-ray applications, since it determines the flux in the focused beam. Moreover, the lens material should generate the lowest intensity of background scattering. The intensity of the background signal observed in the tails of the focused beam (Gasilov et al., 2017[Gasilov, S., Mittone, A., dos Santos Rolo, T., Polyakov, S., Zholudev, S., Terentyev, S., Blank, V., Bravin, A. & Baumbach, T. (2017). J. Synchrotron Rad. 24, 1137-1145.]; Chubar et al., 2020[Chubar, O., Wiegart, L., Antipov, S., Celestre, R., Coles, R., Fluerasu, A. & Rakitin, M. (2020). Proc. SPIE, 11493, 114930M.]) is mainly caused by SAXS (Guinier, 1939[Guinier, A. (1939). Ann. Phys. 11, 161-237.]; Glatter & Kratky, 1982[Glatter, O. & Kratky, O. (1982). Small Angle X-ray Scattering. Academic Press.]), which is primarily due to electron density fluctuations in the scattering volume. The microstructure of the lens material can be either (i) single crystalline like in the diamond lenses presented here, (ii) polycrystalline [for Be lenses (Roth et al., 2014[Roth, T., Helfen, L., Hallmann, J., Samoylova, L., Kwaśniewski, P., Lengeler, B. & Madsen, A. (2014). Proc. SPIE, 9207, 920702.])] or (iii) amorphous [e.g. glassy carbon lenses (Artemiev et al., 2006[Artemiev, A., Snigirev, A., Kohn, V., Snigireva, I., Artemiev, N., Grigoriev, M., Peredkov, S., Glikin, L., Levtonov, M., Kvardakov, V., Zabelin, A. & Maevskiy, A. (2006). Rev. Sci. Instrum. 77, 063113.])]. Additionally, the surface roughness at the air–lens interface also contributes to the total scattering background. It is therefore insightful to compare the SAXS intensities for the different lens materials with that originating from the surface finish. Here we present SAXS measurements for an unpolished and a polished diamond lens, and compare the total scattered intensity to a commercial Be lens manufactured from Materion O30-H grade material. SAXS measurements were carried out at ESRF-EBS beamline ID02 (Narayanan et al., 2018[Narayanan, T., Sztucki, M., Van Vaerenbergh, P., Léonardon, J., Gorini, J., Claustre, L., Sever, F., Morse, J. & Boesecke, P. (2018). J. Appl. Cryst. 51, 1511-1524.]) using an incident X-ray energy of 12.23 keV, corresponding to a wavelength λ = 1.013 Å. In order to cover a wide q range, 0.002 ≤ q ≤ 2 nm−1 (q is the magnitude of the scattering vector given by [q = 4\pi/\lambda\sin{\theta/2}], where θ is the scattering angle), three different sample-to-detector distances were used: 31 m, 8 m and 1 m. The 2D scattering patterns were recorded using an Eiger2 4M detector with an active area of 155.1 mm × 162.2 mm and a pixel size of 75 µm × 75 µm. Fig. 17[link] shows the 2D SAXS pattern acquired at an 8 m sample-to-detector distance for the unpolished diamond (left), the polished diamond (middle) and the reference O30-H Be lens (right). The SAXS signal was recorded with the X-ray beam centred on the thinnest part of each lens. The beam size on the sample was approximately 100 µm × 100 µm, with a photon flux on the order of 6.7 × 1011 photons s−1.

[Figure 17]
Figure 17
Raw 2D detector images showing the SAXS signal of an unpolished (left) and a polished (middle) diamond lens, and an O30-H Be lens (right), taken at a lens-to-detector distance of 8 m with an exposure time of 0.5 s.

Fig. 17[link] shows that the polished diamond lens exhibits a lower background than the unpolished counterpart and also less than the Be reference lens. Additionally, the scattering of the unpolished lens appears highly anisotropic. As the scattering of the polished lens is isotropic, we relate the strong anisotropy to the surface condition before laser polishing. Possible explanations could be that (i) the craters created by the laser ablation process are not radially symmetric, which might be the case if the focused laser beam is not circular in shape or that (ii) sub-micrometre scale surface texture is introduced by the linear polarization of the laser beam as in laser-induced periodic surface structuring (Granados et al., 2017[Granados, E., Martinez-Calderon, M., Gomez, M., Rodriguez, A. & Olaizola, S. M. (2017). Opt. Express, 25, 15330-15335.]). Once this surface layer is removed (polished lens), the crater structure disappears and with it the asymmetric intensity distribution. Finally, the total scattering background of the polished diamond lens becomes low enough so that the crystalline nature of diamond becomes visibly represented by characteristic Kossel lines [see Fig 17 [link](middle)]. Despite the observed anisotropy in the 2D SAXS of the unpolished diamond lens, we performed a full azimuthal integration. The obtained normalized 1D intensities, I(q), are plotted in Fig. 18[link].

[Figure 18]
Figure 18
1D SAXS intensities for the three investigated lenses compared with the empty background. Note that the raw signal for the unpolished diamond lenses in Fig. 17[link] exhibits a large anisotropy. In the azimuthally averaged data a correlation peak appears at q = 0.045 nm−1. Due to the undetermined thickness of the lenses the normalized intensity I(q) is given in steradian−1.

The lower SAXS signal after polishing the laser-ablated diamond lenses is striking. Throughout most of the plotted q-range, the red curve is almost two orders of magnitude lower than the curves of the unpolished diamond lens and of the O30H-grade Be lens. Note that there are Be grades which can yield lower SAXS signals (IF-1, IF-5 and IS50M), though this will improve the situation only by about one order of magnitude (Roth et al., 2014[Roth, T., Helfen, L., Hallmann, J., Samoylova, L., Kwaśniewski, P., Lengeler, B. & Madsen, A. (2014). Proc. SPIE, 9207, 920702.]). The correlation peak in the azimuthally averaged data at q = 0.045 nm−1 of the unpolished lens is still visible in the polished lens, but much reduced. Via 2π/q we obtain a characteristic spacing of 140 nm, which could be well explained by the aforementioned periodic structuring during the laser ablation process.

9. Conclusions

In this paper, we have presented single-crystalline bi-concave 2D focusing diamond lenses that are comparable in quality to commercial Be lenses. These diamond lenses were produced via femtosecond laser ablation followed by a mechanical polishing step. This reduces the surface roughness to an extent that the polished lenses yield a much reduced SAXS background. Focusing capabilities and lens figure errors are very close to those obtained by equivalent Be lenses. We measured the figure errors of the diamond lenses of 1 µm r.m.s. over the full useful lens aperture of almost 400 µm.

Whether single-crystalline HPHT diamond is required or cheaper sc-CVD or polycrystalline grades can be used and give similar quality lenses will be investigated in future measurements. In that case, larger thickness crystals (e.g. 1 mm-thick as common for Be lenses) could allow an increase of the physical aperture or reduction of the lens radius while maintaining the current physical aperture.

The diamond lenses presented here are mounted in common 12 mm-diameter lens frames and feature a reduced frame thickness of 1.2 mm, which can be beneficial for high-energy focusing applications as the total lens stack length can be reduced.

As noted by Serebrennikov et al. (2016[Serebrennikov, D., Clementyev, E., Semenov, A. & Snigirev, A. (2016). J. Synchrotron Rad. 23, 1315-1322.]), diamond lenses are the material of choice for X-ray lenses at higher X-ray energies, i.e. above 30 keV, when the advantage of higher transmission and larger effective aperture of Be lenses decreases. Using diamond and keeping the lens radius equal, only about half the number of lenses are required. At lower energies, diamond lenses have strong potential for applications where the lenses are subjected to high powers or intense short-duration X-ray pulse energies. Future tests of the frame-mounted diamond lens performance when subjected to such illumination conditions will be helpful to show the predicted excellent thermal performance of diamond under white beam conditions and/or resistance to single-pulse X-ray ablation.

APPENDIX A

Refractive index of diamond and beryllium

The focal length of a stack of bi-concave X-ray lenses can be well approximated by f = R/(2Nδ), where R is the radius of curvature, N is the number of lenses and δ is the refractive index decrement. Fig. 19[link] shows δC* and δBe and their ratio for energies ranging from 5 keV to 50 keV. The mean value of this ratio is 2.14 with less than 0.5% variation in the whole energy range.

[Figure 19]
Figure 19
Index of refraction decrement (top) calculated using the xraylib library (Brunetti et al., 2004[Brunetti, A., Sanchez del Rio, M., Golosio, B., Simionovici, A. & Somogyi, A. (2004). At. Spectrosc. 59, 1725-1731.]) and their ratio (bottom).

Footnotes

Now at: Palm Scientific, Naperville, IL 60565, USA.

Acknowledgements

We acknowledge the ESRF for providing beam time on ID02, BM05 and ID06. We thank Philip Cook, Luca Capasso and Carsten Detlefs for help with setting up beamlines BM05 and ID06. We thank Sebastian Berujon and Ruxandra Cojocaru for discussions and initial help with the XSVT data analysis code.

Funding information

RC acknowledges funding from the European Union's Horizon 2020 research and innovation programme (grant agreement No. 101007417) within the framework of the NFFA-Europe Pilot Joint Activities. SA acknowledges funding from US DOE SBIR program (grant No. DE-SC0013129).

References

First citationAlianelli, L., Sawhney, K. J. S., Malik, A., Fox, O. J. L., May, P. W., Stevens, R., Loader, I. M. & Wilson, M. C. (2010). J. Appl. Phys. 108, 123107.  Web of Science CrossRef Google Scholar
First citationAndrejczuk, A., Krzywiński, J., Sakurai, Y. & Itou, M. (2010). J. Synchrotron Rad. 17, 616–623.  Web of Science CrossRef CAS IUCr Journals Google Scholar
First citationAntipov, S., Assoufid, L., Grizolli, W., Qian, J. & Shi, X. (2018). Proceedings of the 9th International Particle Accelerator Conference (IPAC'18), 29 April–4 May 2018, Vancouver, BC, Canada, pp. 4057–4058. THPMF011.  Google Scholar
First citationAntipov, S., Baryshev, S. V., Butler, J. E., Antipova, O., Liu, Z. & Stoupin, S. (2016). J. Synchrotron Rad. 23, 163–168.  Web of Science CrossRef CAS IUCr Journals Google Scholar
First citationArtemiev, A., Snigirev, A., Kohn, V., Snigireva, I., Artemiev, N., Grigoriev, M., Peredkov, S., Glikin, L., Levtonov, M., Kvardakov, V., Zabelin, A. & Maevskiy, A. (2006). Rev. Sci. Instrum. 77, 063113.  Web of Science CrossRef Google Scholar
First citationBerujon, S., Cojocaru, R., Piault, P., Celestre, R., Roth, T., Barrett, R. & Ziegler, E. (2020a). J. Synchrotron Rad. 27, 293–304.  Web of Science CrossRef IUCr Journals Google Scholar
First citationBerujon, S., Cojocaru, R., Piault, P., Celestre, R., Roth, T., Barrett, R. & Ziegler, E. (2020b). J. Synchrotron Rad. 27, 284–292.  Web of Science CrossRef IUCr Journals Google Scholar
First citationBrunetti, A., Sanchez del Rio, M., Golosio, B., Simionovici, A. & Somogyi, A. (2004). At. Spectrosc. 59, 1725–1731.  Web of Science CrossRef Google Scholar
First citationCelestre, R., Berujon, S., Roth, T., Sanchez del Rio, M. & Barrett, R. (2020a). J. Synchrotron Rad. 27, 305–318.  Web of Science CrossRef IUCr Journals Google Scholar
First citationCelestre, R., Chubar, O., Roth, T., Sanchez del Rio, M. & Barrett, R. (2020b). Proc. SPIE, 11493, 114930J.  Google Scholar
First citationCheng, J., Liu, C., Shang, S., Liu, D., Perrie, W., Dearden, G. & Watkins, K. (2013). Opt. Laser Technol. 46, 88–102.  Web of Science CrossRef Google Scholar
First citationChubar, O., Berman, L., Chu, Y. S., Fluerasu, A., Hulbert, S., Idir, M., Kaznatcheev, K., Shapiro, D., Shen, Q. & Baltser, J. (2011). Proc. SPIE, 8141, 814107.  CrossRef Google Scholar
First citationChubar, O. & Elleaume, P. (1998). Proceedings of the 6th European Particle Accelerator Conference (EPAC'98), 22–26 June 1998, Stockholm, Sweden, pp. 1177–1179. THP01G.  Google Scholar
First citationChubar, O., Wiegart, L., Antipov, S., Celestre, R., Coles, R., Fluerasu, A. & Rakitin, M. (2020). Proc. SPIE, 11493, 114930M.  Google Scholar
First citationDhamgaye, V., Laundy, D., Baldock, S., Moxham, T. & Sawhney, K. (2020). J. Synchrotron Rad. 27, 1518–1527.  Web of Science CrossRef CAS IUCr Journals Google Scholar
First citationFox, O. J. L., Alianelli, L., Malik, A. M., Pape, I., May, P. W. & Sawhney, K. J. S. (2014). Opt. Express, 22, 7657–7668.  Web of Science CrossRef CAS PubMed Google Scholar
First citationGasilov, S., Mittone, A., dos Santos Rolo, T., Polyakov, S., Zholudev, S., Terentyev, S., Blank, V., Bravin, A. & Baumbach, T. (2017). J. Synchrotron Rad. 24, 1137–1145.  CrossRef CAS IUCr Journals Google Scholar
First citationGlatter, O. & Kratky, O. (1982). Small Angle X-ray Scattering. Academic Press.  Google Scholar
First citationGranados, E., Martinez-Calderon, M., Gomez, M., Rodriguez, A. & Olaizola, S. M. (2017). Opt. Express, 25, 15330–15335.  Web of Science CrossRef CAS PubMed Google Scholar
First citationGuinier, A. (1939). Ann. Phys. 11, 161–237.  CrossRef Google Scholar
First citationIsakovic, A. F., Stein, A., Warren, J. B., Narayanan, S., Sprung, M., Sandy, A. R. & Evans-Lutterodt, K. (2009). J. Synchrotron Rad. 16, 8–13.  Web of Science CrossRef CAS IUCr Journals Google Scholar
First citationJJ-X-ray (2021). Single Crystal Diamond Compound Refractive Lenses, https://www.jjxray.dk/p/xx-single-crystal-diamonds/Google Scholar
First citationKohn, V. G. (2017). J. Synchrotron Rad. 24, 609–614.  Web of Science CrossRef CAS IUCr Journals Google Scholar
First citationKononenko, T. V., Ralchenko, V. G., Ashkinazi, E. E., Polikarpov, M., Ershov, P., Kuznetsov, S., Yunkin, V., Snigireva, I. & Konov, V. I. (2016). Appl. Phys. A, 122, 152.  Web of Science CrossRef Google Scholar
First citationKutsal, M., Bernard, P., Berruyer, G., Cook, P. K., Hino, R., Jakobsen, A. C., Ludwig, W., Ormstrup, J., Roth, T., Simons, H., Smets, K., Sierra, J. X., Wade, J., Wattecamps, P., Yildirim, C., Poulsen, H. F. & Detlefs, C. (2019). Mater. Sci. Eng. 580, 012007.  Google Scholar
First citationLengeler, B. (2012). Refractive X-ray Lenses: New Developments. Presentation. RWTH Aachen and RXOPTICS, Germany (https://www.rxoptics.de/wp-content/uploads/2018/12/RXOPTICS-Lecture-2012.pdf).  Google Scholar
First citationLengeler, B. & Lengeler, D. (2021). RXOPTICS, Germany (https://www.rxoptics.de).  Google Scholar
First citationLengeler, B., Schroer, C., Tümmler, J., Benner, B., Richwin, M., Snigirev, A., Snigireva, I. & Drakopoulos, M. (1999). J. Synchrotron Rad. 6, 1153–1167.  Web of Science CrossRef IUCr Journals Google Scholar
First citationLyubomirskiy, M., Boye, P., Feldkamp, J. M., Patommel, J., Schoeder, S., Schropp, A., Burghammer, M., Wild, C. & Schroer, C. G. (2019). J. Synchrotron Rad. 26, 1554–1557.  Web of Science CrossRef CAS IUCr Journals Google Scholar
First citationMalik, A. M., Fox, O. J. L., Alianelli, L., Korsunsky, A. M., Stevens, R., Loader, I. M., Wilson, M. C., Pape, I., Sawhney, K. J. S. & May, P. W. (2013). J. Micromechan. Microeng. 23, 125018.  Web of Science CrossRef Google Scholar
First citationMedvedskaya, P., Lyatun, I., Shevyrtalov, S., Polikarpov, M., Snigireva, I., Yunkin, V. & Snigirev, A. (2020). Opt. Express, 28, 4773–4785.  Web of Science CrossRef PubMed Google Scholar
First citationNarayanan, T., Sztucki, M., Van Vaerenbergh, P., Léonardon, J., Gorini, J., Claustre, L., Sever, F., Morse, J. & Boesecke, P. (2018). J. Appl. Cryst. 51, 1511–1524.  Web of Science CrossRef CAS IUCr Journals Google Scholar
First citationNöhammer, B., David, C., Rothuizen, H., Hoszowska, J. & Simionovici, A. (2003). Microelectron. Eng. 67–68, 453–460.  Google Scholar
First citationNöhammer, B., Hoszowska, J., Freund, A. K. & David, C. (2003b). J. Synchrotron Rad. 10, 168–171.  Web of Science CrossRef IUCr Journals Google Scholar
First citationOsellame, R., Cerullo, G. & Ramponi, R. (2012). Editors. Femto­second Laser Micromachining, Vol. 123 of Topics in Applied Physics. Springer Science & Business Media.  Google Scholar
First citationOsterhoff, M., Detlefs, C. & Ferrero, C. (2017). Proc. SPIE, 10388, 103880L.  Google Scholar
First citationPolikarpov, M., Polikarpov, V., Snigireva, I. & Snigirev, A. (2016). Phys. Proc. 84, 213–220.  CrossRef CAS Google Scholar
First citationRoth, T., Helfen, L., Hallmann, J., Samoylova, L., Kwaśniewski, P., Lengeler, B. & Madsen, A. (2014). Proc. SPIE, 9207, 920702.  Google Scholar
First citationSanchez del Rio, M. & Alianelli, L. (2012). J. Synchrotron Rad. 19, 366–374.  Web of Science CrossRef IUCr Journals Google Scholar
First citationSchroer, C. G., Kuhlmann, M., Lengeler, B., Gunzler, T. F., Kurapova, O., Benner, B., Rau, C., Simionovici, A. S., Snigirev, A. A. & Snigireva, I. (2002). Proc. SPIE, 4783, 10–18.  CrossRef CAS Google Scholar
First citationSeiboth, F., Brückner, D., Kahnt, M., Lyubomirskiy, M., Wittwer, F., Dzhigaev, D., Ullsperger, T., Nolte, S., Koch, F., David, C., Garrevoet, J., Falkenberg, G. & Schroer, C. G. (2020). J. Synchrotron Rad. 27, 1121–1130.  Web of Science CrossRef CAS IUCr Journals Google Scholar
First citationSerebrennikov, D., Clementyev, E., Semenov, A. & Snigirev, A. (2016). J. Synchrotron Rad. 23, 1315–1322.  Web of Science CrossRef CAS IUCr Journals Google Scholar
First citationShvyd'ko, Y., Blank, V. & Terentyev, S. (2017). MRS Bull. 42, 437–444.  Google Scholar
First citationSnigirev, A. A., Yunkin, V., Snigireva, I., Di Michiel, M., Drakopoulos, M., Kouznetsov, S., Shabel'nikov, L., Grigoriev, M., Ralchenko, V., Sychov, I., Hoffmann, M. & Voges, E. I. (2002). Proc. SPIE, 4783, 1–9.  CrossRef CAS Google Scholar
First citationSnigirev, A., Kohn, V., Snigireva, I. & Lengeler, B. (1996). Nature, 384, 49–51.  CrossRef CAS Web of Science Google Scholar
First citationSugioka, K. & Cheng, Y. (2014). Light Sci. Appl. 3, e149.  Web of Science CrossRef Google Scholar
First citationTerentyev, S., Blank, V., Polyakov, S., Zholudev, S., Snigirev, A., Polikarpov, M., Kolodziej, T., Qian, J., Zhou, H. & Shvyd'ko, Y. (2015). Appl. Phys. Lett. 107, 111108.  Web of Science CrossRef Google Scholar
First citationTerentyev, S., Polikarpov, M., Snigireva, I., Di Michiel, M., Zholudev, S., Yunkin, V., Kuznetsov, S., Blank, V. & Snigirev, A. (2017). J. Synchrotron Rad. 24, 103–109.  Web of Science CrossRef CAS IUCr Journals Google Scholar
First citationTomie, T. (1997). X-ray lens. US Patent US5594773A, filed February 1995.  Google Scholar
First citationZhu, T.-F., Fu, J., Wang, W., Wen, F., Zhang, J., Bu, R., Ma, M. & Wang, H.-X. (2017). Opt. Express, 25, 1185–1192.  Web of Science CrossRef CAS PubMed Google Scholar
First citationZiegler, E. (2004). AIP Conf. Proc. 705, 436–439.  CrossRef Google Scholar

This is an open-access article distributed under the terms of the Creative Commons Attribution (CC-BY) Licence, which permits unrestricted use, distribution, and reproduction in any medium, provided the original authors and source are cited.

Journal logoJOURNAL OF
SYNCHROTRON
RADIATION
ISSN: 1600-5775
Follow J. Synchrotron Rad.
Sign up for e-alerts
Follow J. Synchrotron Rad. on Twitter
Follow us on facebook
Sign up for RSS feeds