research papers
In situ XAFS–XRD study of the Zr–Y2O3 interaction at extra-high temperatures
aLaboratory for Zero-Carbon Energy, Tokyo Institute of Technology, 2-12-1 N1-3 Ookayama, Meguro-ku, Tokyo 152-8550, Japan, bInstitute of Materials Research, Tohoku University, 2145-2 Narita-cho, Oarai-cho, Ibaraki-gun, Ibaraki 311-1313, Japan, cResearch Institute of Nuclear Engineering, University of Fukui, 1-3-33 Tetsuwa-cho, Tsuruga-shi, Fukui 914-0055, Japan, and dMaterials Science Research Center, Japan Atomic Energy Agency, 1-1-1 Kouto, Sayo-cho, Sayo-gun, Hyogo 679-5148, Japan
*Correspondence e-mail: itoh.a.ae@m.titech.ac.jp
The in situ measurement technique for a metal/metal-oxide mixture at extra-high temperature above 2000 K has been desired in the field of nuclear safety engineering. In the present study, we succeeded in simultaneous XAFS–XRD measurements of the Zr oxidation [Zr + O → Zr(O) + ZrO2] up to 1952 K and ZrO2–Y2O3 reaction from 1952 to 2519 K. The during Zr oxidation was observed in the absorption spectra around the Zr K-edge, and the interatomic cation–cation and cation–oxygen distances obtained by the fitting analysis of during the Y2O3–ZrO2 reaction are explained. Also, the temperature dependency of the anharmonic effect was investigated by comparing the fitted second- and third-order cumulants with the theoretical ones in which the Morse potential was applied as an interatomic potential, giving a good explanation about the local structure dynamics. Finally, the applicability of the developed system to investigation of materials, such as UO2–Zr, is discussed.
Keywords: in situ XAFS–XRD; Zr–Y2O3; extra-high temperature.; Zr–Y2O3.
1. Introduction
For the safety evaluation of 2–Zr diffusion couples were heated to a target temperature using an induction furnace, held for a certain period of time, cooled to room temperature, and then the samples were chemically analyzed to evaluate the extent of the reaction. According to the results, it has been reported that the melting amount of UO2 in Zr rapidly proceeds above approximately 2273 K (Hofmann & Politis, 1979; Tim & Olander, 1988; Kim & Olander, 1988; Hayward & George, 1994, 1996; Hayward et al., 1999; Shirasu et al., 2023). However, the analytical results obtained by such a method include large uncertainties derived from reactions during the heating and cooling processes, and thus it is difficult to estimate the precise chemical conditions in which the melting reaction begins. To elucidate the state of the materials and the intrinsic physicochemical state at high temperature, in situ observation techniques using synchrotron radiation have attracted attention.
materials, it is important to obtain knowledge on the high-temperature reactions that cause fuel-cladding melting. In previous fuel-melting experiments, UOX-ray absorption fine structure (XAFS) is a technique for investigating the local atomic structure in both solid and liquid phases and has been successfully applied to many types and states of materials. Recently, et al., 2017) and molten salts at high temperatures (Bessada et al., 2017, 2020). In situ X-ray diffraction (XRD) measurement is also a powerful technique for tracing structural transitions during heat treatment and has been applied to molten UO2 coupled with the laser ablation method (Skinner et al., 2014). These two techniques complement each other, and coupling with XRD has often been applied for investigation of the reaction kinetics of functional materials (such as catalysts). However, few studies have been reported on the application of the combined XAFS–XRD technique at high temperature.
has been applied to nuclear materials, such as molten rare-earth oxides (OkamotoIn the present study, we focus on the in situ XAFS–XRD technique to investigate the high-temperature interaction (above 2000 K) of Zr–Y2O3 mixture by additionally installing XRD apparatus to the measurement system developed by one of authors (Niino et al., 2023). Firstly, the temperature of the sample was calibrated using a heating test with the Y2O3 powder from room temperature to approximately 2700 K. Thereafter, a specimen of Zr–Y2O3 (Zr:Y2O3 = 50:50 wt%) was prepared and then heated up to approximately 2500 K. The X-ray absorption and diffraction images from the transmitted X-rays were recorded, which enabled phase relations and the local structures around metals (Y and Zr) to be studied. Our results are compared with the literature regarding the Y2O3 and ZrO2–Y2O3 system to check the validity of the improved system, and then its applicability to the Zr–UO2 interaction in the future is discussed.
2. Experimental procedure
2.1. Measurement system
Fig. 1 shows a schematic diagram of the XAFS–XRD measurement system. We installed the heating chamber and collected the and XRD data at beamline BL22XU (Shobu et al., 2007) at SPring-8 (Hyogo, Japan), which can generate X-rays with energies in the range 5–70 keV. A monochromator crystal of Si(111), equipped in a cam-type double-crystal monochromator (Kohzu Precision Co. Ltd) (Yabashi et al., 1999), was utilized for obtaining the X-rays for measurement. In this study, X-rays with energies in the range 16.839–18.561 keV were used. A nickel-coated mirror (bent cylindrical mirror with glancing angle of 1.9 mrad) installed downstream of the monochromator focused the X-rays and rejected higher harmonics, and another nickel-coated flat mirror returned the beam direction to horizontal. In the measurement, at first, X-rays with an energy of 17.72 keV transmitted through the sample were captured by a 1024 × 1024 pixel CCD area detector (Hamamatsu Photonics KK) to obtain the diffraction image. For in transmission, the monochromator was quick-scanned between 16.839 and 18.561 keV to cover both the Y K-edge (17.038 keV) and the Zr K-edge (17.998 keV). The data collection time was 20 s for and 10 s for the diffraction image at each temperature. The X-ray beams were focused to an area of approximately 0.4 mm2 and the measurements were performed in the transmission mode using two ionization chambers (IC#1, IC#2) filled with nitrogen gas to count the photons absorbed by the sample. The specimens with sample material (prepared as explained in the next section) were placed in a stainless-steel heating chamber. The chamber had two quartz-glass windows of thickness 6 mm and diameter 60 mm for pyrometer use. Each glass window had a hole at the center and the hole was covered with polyimide film (0.069 mm in thickness). The X-ray beam passed through the polyimide film. Sample material was placed in the slit of a tungsten sample holder. Electrodes attached to the sample holder were connected to a programmable DC power supply (TAKASAGO Ltd) (0–6 V, 0–400 A) to enable effective heating of the sample materials. The temperature of the sample was monitored by a one-color pyrometer (LUMASENSE IGA 740-LO). The temperature measuring spot was 1.5 mm at a distance of 300 mm, which covered the tungsten holder around the sample. The temperature reached using the pyrometer was corrected by an W-Re type thermocouple; however, uncertainty inevitably arises above approximately 2273 K. Therefore, the temperature was corrected with the lattice parameter of Y2O3 as explained in Section 3.1. At the beginning of the measurement, the chamber was filled with pure argon gas (99.9999% purity) and vacuumed at ∼104 Pa. Details of the sample holder are given by Niino et al. (2023) and shown in Fig. S1 of the supporting information.
2.2. Sample preparation
Specimens were prepared by mixing Y2O3 powder (99.99% purity, Kojundo Chemical Laboratory Co. Ltd) and isopropyl alcohol (extra-pure reagent, Kanto CHEMICAL Co. Inc.) in a mortar to produce a slurry. To test the Zr–Y2O3 mixture (Zr:Y2O3 = 50:50 wt%), Zr powder (99.9% purity, FUJIFILM Wako Pure Chemical Co. Ltd) was mixed with Y2O3 powder. The slurry sample was pasted onto the slit (60 µm wide) of the W holder, dried, and stabilized by heating at 673 K for 20 h. All preparations were conducted in an inert After the XAFS–XRD measurements, the specimens were removed from the heating chamber. Then metallographic analyses were performed via with electron dispersion spectroscopy (SEM/EDS; JSM-6010 LV, Jeol) and with a spherical aberration corrector (AC-TEM; ARM 200F, Jeol) to investigate the final state of the sample materials.
2.3. Data analysis
The diffraction images were transformed into intensity profiles using IPAnalyzer software (Seto et al., 2010). Diffraction patterns from the irradiated X-ray energy in this study (17.72 keV) were calculated using RIETAN software (Kim & Izumi, 1994), and the peaks were compared with the experimental ones of Swamy et al. (1999).
The K-edges were analyzed using the Athena software to extract the function (Ravel & Newville, 2005), χ(k), expressed as
spectra at the Y and Zrwhere k is the photoelectron wavenumber, ℏ (= h/2π) is the reduced Plank constant, m is the mass of an electron, E is the energy of the incident X-rays, E0 is the point at which the second-order derivative with respect to energy is zero, μ(k) is the total μb(k) is the background contribution from the excitations of other shells and atoms in the sample, and μ0(k) is calculated by a least-square fitting with the Victoreen's formula aE−3 − bE−4 − c (where a, b and c are constants). The Hamming window function was multiplied by χ(k) to avoid the truncation error in the Fourier transformed spectra in R-space. The k-range for the Fourier transform was from 3 to 10. We obtained the radial structural function (RSF) from the k3-weighted Fourier transformed magnitude |FT[k3χ(k)]| with the function, which were further used to obtain parameters of local structure (coordination number, interatomic distance, Debye–Waller factor and third-order cumulant) by curve fitting analysis with the Artemis software (Ravel & Newville, 2005) with the following formula,
where Ri is the interatomic distance between absorbing and photoelectron scattering atom i, Ni is the f(k, Ri) and ϕ(k) are the backscattering amplitude and total phase shift functions [which were calculated by FEFF6 code (Rehr & Ankudinov, 2001) embedded in the Artemis software], λ is the photoelectron is the second-order cumulant (arising mainly from the harmonic part in the interatomic potential), and C3,i is the third-order cumulant (giving the anharmonic effect in the interatomic potential). It should be noted that the fourth-order cumulant is also essential in the analysis at ultra-high temperature, because it may affect the amplitude of χ(k) reflecting the anharmonic effect. However, it was difficult to obtain good fitting results with the spectra in this study due to the insufficient signal-to-noise (S/N) ratio at high k-range. Therefore, we performed the analysis only up to the third-order cumulant. The S0 2 value was firstly determined from the spectrum taken at 300 K (before heating) and was used as fixed values for other temperatures' fitting analysis.
3. Results
3.1. Temperature calibration with Y2O3 measurements
The X-ray patterns obtained at seven different powers (0, 78, 100, 148, 193, 205 and 282 W) are shown in Fig. 2. The peak labeled Y(hkl) represents cubic Y2O3 in the and Yh(hkl) represents monoclinic Y2O3 in the C2/m, which was formed in the temperature range 2500–2600 K (Jacobson et al., 2004). The diffraction spectrum at 300 K (P = 0) exhibited a Debye ring at 2θ = 13.09°, which was identical to that of cubic Y2O3 calculated using the RIETAN code with the (CIF) (Andrievskaya et al., 1996) obtained via AtomWork (https://crystdb.nims.go.jp/) (Xu et al., 2011). The corresponding d-spacing and unit-cell parameter were calculated as 3.06 and 10.6031 Å, respectively. The peak of the d-spacing at high temperature shifted to 3.13 Å (Table 1). Above P = 200 W, the Debye ring disappeared, and spots appeared at P = 282 W [Fig. 2(b)]. 2θ of these peaks corresponds to the Bragg diffraction of monoclinic Y2O3 (Skrikanth et al., 1994). Immediately after that spot was observed, it disappeared from the diffraction image. At the same time, attenuation in the X-ray absorption was also observed. Based on this observation, the sample was considered to have been in a coarse-grained state at the temperature of the phase transformation from the cubic structure (∼2530 K) to the melting point (2712 K). We note that the diffraction peak width clearly changed at the temperature; the broad peak in the low-temperature phase [Fig. 2(a)] shrinked to almost the resolution limit in the high temperature phase [Fig. 2(b)]. The reason for this is not clear, but the sample crystal could be strained during the sample preparation.
|
Unit-cell parameters up to P = 205 W were used to estimate the temperatures applied in this study. Fig. 3 shows the unit-cell parameters of cubic Y2O3 at 300–2530 K as a function of temperature, as investigated by Swamy et al. (1999). The temperatures at each power level were estimated, and the obtained values are listed in Table 1. By adding the melting point of Y2O3 at 282 W, the following second-order polynomial was obtained,
where T is the temperature and P is the power applied to the specimen. The estimated temperatures against the power using the fitting curve are shown in Fig. 4.
The et al., 2020) in which the discontinuously dropped due to a drastic change of absorbing atom density. Fig. 5 shows selected X-ray absorption spectra, indicating that the Yh structure also exhibited low absorption (P = 280 W). The absorption differences from 300 K at 17.038 keV are plotted against the temperature in Fig. 6. The absorption level was almost constant up to 2400 K and then discontinuously decreased at the points where monoclinic Y2O3 appeared and melted, which is consistent with the observed diffraction pattern.
can be distinguished by examining the absorption difference in the XANES spectra using the T-scan method (Boccato3.2. XAFS–XRD measurement for Zr–Y2O3
3.2.1. XRD profiles and SEM/TEM of the cooled sample
Fig. 7 shows XRD profiles obtained by conversion of diffraction images from 300 to 2561 K. The temperatures were converted to Kelvin using equation (4). Before heating at 300 K, peaks corresponding to cubic Y2O3 and hexagonal Zr were observed. In the diffraction image, a continuous ring was clearly observed for cubic Y2O3, whereas a spotted ring was observed for hexagonal Zr [Fig. 7(a)]. As the temperature increased, the Zr peak became less intense [Fig. 7(b)] and disappeared at 2224 K, whereas the peak of tetragonal ZrO2 appeared at 1674 K and increased with a decrease in the amplitude of the cubic Y2O3 peak. Fig. 7(c) shows the moment at 1952 K at which cubic ZrO2 peak became stronger whereas cubic Y2O3 and hexagonal Zr peaks became weaker. The diffraction image at 2519 K [Fig. 7(d)] shows spots between the two rings (cubic Y2O3 and ZrO2), giving a broad peak in the XRD profile and indicating partial formation of a of Y2O3–ZrO2 (Butz et al., 2006). Fig. 8 shows the XRD pattern obtained after heating test by switching off the current heating, consisting of patterns from cubic Y2O3, cubic ZrO2 and monoclinic ZrO2. SEM/EDS analysis of the cooled sample was performed, as shown in Fig. 9. Three distinct regions were observed: Y–Zr oxide (point 1), Zr-rich oxide (point 2) and Y-rich oxide (point 3). The composition at each point was analyzed by EDS as summarized in Table 2.
|
The TEM analysis of the cooled sample is summarized in Fig. 10. A membrane sample of thickness 150 nm was fabricated using a focused ion milling technique from a large crystal grain corresponding to the point 1: Y2O3–ZrO2 which is shown in Fig. 9. Figs. 10(b) and 10(c) are selected areas where diffraction patterns were obtained at regions (i) and (ii) in a bright-field TEM image shown as Fig. 10(a). It was found that the annealed coarse grain was mainly composed of monoclinic ZrO2 polycrystalline grains and cubic ZrO2 polycrystalline grains. In addition, near the surface of the annealed coarse grain, cubic YZrO2 aggregation containing many nanovoids was observed. Fig. 10(d) is an aberration-corrected TEM (AC-TEM) image along the [110] direction of the cubic YZrO2, which shows an extra spot in the diffraction pattern in Fig. 10(c) (indicated by the arrow). Lattice distances such as d = 0.29 nm and 0.18 nm were almost equal to ones in other cubic ZrO2 grains.
3.2.2. of the Zr-K absorption spectra
The normalized X-ray . The value of E0 at 300 K was calibrated by the spectrum of Zr foil (99.99% purity, Nilaco Co. Ltd) at 17.998 keV. The temperature dependency of E0 is plotted in Fig. 11(a), showing that E0 remained at the level of Zr until 1674 K, shifted continuously to the higher energy range with increasing of temperature to 2041 K, reached the same level as the ZrO2 powder above 2200 K, and then settled at this level thereafter.
was plotted against the energy of the incident X-rays for each temperature as shown in Fig. 113.2.3. spectra during heating and after cooling
We investigated the K-edge with fitting results at 300, 1138, 1251, 1508, 1952, 2224 and 2519 K are plotted in k-space as shown in Fig. 12. With the exception of 300 K, the k3-weighted oscillations were too large to provide appropriate fitting results in the range greater than k = 10. Hence, the range of the Fourier transform was set to the k-range of 3–10 to calculate the RSF (Fig. 13). The curve fitting analysis results are summarized in Table 3.
spectra to understand the local structural changes during the heating process. Extracted oscillations for Zr and Y at the
|
The RSF for Zr-K at 300 K exhibited the first peak at ∼2.9 Å, which is attributable to the contribution of the first coordination shell (Zr—Zr) with the bonding distance of 3.21 Å. The RSF for Y-K exhibited the first peak at ∼1.7 Å owing to the first coordination shell (Y—O, nearest six oxygen atoms) and the second peak at ∼3.58 Å mainly owing to the second coordination shells (Y—Y). Cubic Y2O3 exhibits a variety of peaks owing to the non-equivalent Y atoms, Y1 and Y2 (Jonane et al., 2016). Out of two types of Y—O coordination, one exhibits six equivalent bonding lengths of 2.89 Å and the other exhibits distorted octahedral structure with three groups of slightly different bonding lengths of (2.24, 2.27, 2.33 Å) × 2. The averaged value of the latter groups is 2.27 Å, which was 1.7% smaller than the value of the present study (2.31 Å).
As the temperature increases, the peak intensity of RSF for Zr—Zr decreases and almost disappears at 1952 K, whereas the appearance of the peak at ∼1.5 Å suggests that the first coordination was changed from Zr—Zr to Zr—O. Regarding the RSF for the Y-K edge, the peak intensity of Y—Y decreases above 1508 K and almost disappears at 2224 K.
Fig. 14 shows the RSF of the cooled sample after switching off current-heating. The RSF for Zr-K exhibits three peaks at ∼1.5, ∼2.5 and ∼3.1 Å, arising from the first coordination shell (Zr—O), the second and third coordination shells (Zr—Zr), respectively. The interatomic distances for each shell are close to the averaged bonding length of Zr—O in monoclinic ZrO2 (2.16 Å), Zr—Zr in monoclinic ZrO2 (3.44 Å) and Zr—Zr in cubic ZrO2 (3.63 Å). The RSF for Y-K exhibited several peaks in the R-range of 1–6 Å; however, we performed fitting analysis against the second and third peaks from 1.2 to 4 Å because the first peak at ∼1 Å probably appeared as a truncation error of the Fourier transformed calculation. Obtained interatomic distances were 2.33 Å for Y—O and 3.64 Å for Y—Y, respectively, which were slightly larger than the averaged bonding length of cubic Y2O3.
4. Discussion
4.1. Phase transitions and local structure change during the heating process
Based on the XRD patterns (Fig. 7), ZrO2 was formed above 1674 K and coexisted with Zr up to 2041 K. In this temperature range, the E0 shows a continuous shift to higher energy range, indicating that Zr was gradually oxidized. Since hexagonal Zr can dissolve oxygen up to ∼30 at% according to the Zr—O phase diagram (Arroyave et al., 2002), oxygen-dissolved Zr [i.e. α-Zr(O)] coexisted with ZrO2. Hence, the X-ray absorption could have contributions from α-Zr(O) and ZrO2, then exhibit a gradual change. This interpretation can explain the interatomic distance of Zr—Zr shown in Fig. 15(a), which gradually increases as temperature increases above 1500 K. Oxidation may have been caused by the residual oxygen in the furnace, not by reducing Y2O3 because the equilibrium oxygen of Y is much lower than that of Zr (Kleykamp, 1985).
At 1952 K, the reaction between ZrO2 and Y2O3 could have commenced, affecting the RSF of Y-K in which the peak for Y—Y shells mostly disappeared. Tuilier et al. (1987) observed similar behavior when investigating the Y2O3–ZrO2 reaction annealed at 1700–1800°C. Above 1952 K, the interatomic distance of Y—Y and Y—O obtained by the analysis shows increasing tendency with large fluctuation [Figs. 15(a) and 15(b)] and the of Y—Y decreased from 12.0 to 8.6 (Table 3). The Zr—O distance [Fig. 15(b)] also shows large fluctuations, which may arise from the low S/N ratio of the measurement data. The constraint for fitting of the third-order cumulant could have affected the interatomic distance, causing such fluctuation. This result was also observed in the study of ZrO2-doped yttria (Duraud et al., 1990; Thromat et al., 1991). Those authors suggested that a small value of the second cumulant and a large oxygen deficit around Y contradicted the theory of vacancy formation in Y2O3-doping into ZrO2 [it is well known that when Y2O3 is dissolved in ZrO2 an oxide defect could be formed to compensate for the electrical charge because the trivalent Y has a negative charge on the tetravalent Zr, and the oxide defects tend to gather around Zr, not Y (Ando & Oishi, 1985)]. Others investigated the site selectivity in ZrO2-doped Y2O3 by spectra calculation (Crocombette & Jollet, 1994), stating that Zr could tend to more probably substitute for Y2 than for Y1, although the relation between their conclusion and the large oxide defect for Y—O is still unknown. This different observation between ZrO2-doped Y2O3 and Y2O3-doped ZrO2 could be caused by a different defect formation mechanism. The possibility of an oxygen deficit around the metal atom in ZrO2-doping reactions is important in our target system (U—Zr—O) because the interaction between metal and oxygen-deficient metal could promote eutectic melting. From this point of view, the present study is valuable for future work.
4.2. Influence of anharmonic phonon oscillations on the local structure
At high temperature, anharmonic effects in the interatomic potential cannot be neglected in temperature-dependent ), who calculated the temperature dependency of the second- and third-order cumulant for the diatomic model in which the Morse potential, V(x), is assumed as the interatomic potential, as
studies. In the present study, the temperature dependencies of the obtained second- and third-order cumulants were analyzed by comparison with the theoretical ones proposed by Miyanaga & Fujikawa (1994where σ2 is the second-order cumulant, C3 is the third-order cumulant, D and α are parameters in the Morse potential, a is the interatomic distance between the absorbing and scattering atoms, kB is the and T is temperature. As described in the equations, σ2 arising mainly from harmonic phonon oscillation varies linearly on T reflecting attenuation of the amplitude, while C3 from anharmonic effects depends on T2 reflecting the asymmetry of the interatomic distance distribution (deviation from the symmetric Gaussian distribution).
Figs. 16 and 17 show the variation of σ2 and C3 with T for cation–cation and cation–oxygen couples. For the cation–cation couples, σ2 of Y—Y tended to increase linearly, whereas that of Zr—Zr increased linearly up to approximately 1500 K and then decreased [Fig. 16(a) circled as A]. This may be because oxidation of Zr somehow stabilized Zr—Zr bonding. The values of C3 exhibited the tendency to increase as shown in Fig. 16(b). Positive values of the third-order cumulant means that the interatomic distance distribution has more weight on the longer bonds. Hence, this behavior is consistent for longer interatomic distances at high temperatures. For the cation–oxygen couples, σ2 for Y—O clearly showed a tendency to linearly increase up to approximately 2000 K, whereas σ2 of Zr—O and Y—O above 2000 K tended to decrease [Fig. 17(a) circled as A], although some points for Y—O showed a tendency to increase. This behavior might be attributable to stabilization of bonds due to the ZrO2–Y2O3 reaction. On the other hand, as shown in the cation–cation shell, C3 of Y—O and Zr—O showed an increase with temperature. This is also consistent with the tendency shown in the interatomic distance for the cation–oxygen shell which increase as temperature increased. Based on these observations, the fits applying the diatomic theory proposed by Miyanaga & Fujikawa (1994) qualitatively explained the high-temperature interaction in the present study. Also, it was found that thermal disorder above 2000 K from the ZrO2–Y2O3 reaction was caused mostly by anharmonic effects.
4.3. State of the cooled sample after the heating process
The specimen was rapidly quenched by switching off the current-heating. Therefore, part of the high-temperature state could have remained in the cooled sample. The SEM image in Fig. 9 shows three distinct regions: Y–Zr oxide (point 1), Zr-rich oxide (point 2) and Y-rich oxide (point 3), which is consistent with the XRD patterns of the cooled sample as shown in Fig. 8. The broad peak-top splitting pattern from 13.17 to 13.54° suggests that the Y2O3–ZrO2 reaction formed polycrystalline forms of (Y, Zr)O2–x with various Y/Zr ratios, which is also consistent with the TEM analysis result as shown in Fig. 10(a). A number of and defects were observed in the cubic YZrO2 grain, especially near nanovoids. Since an extra spot in Fig. 10(c) (noted by the arrow) was a point which did not appear by the extinction rule, the YZrO2 structure was probably not a `perfect cubic' structure (Butz et al., 2006). This result means that some of the Y2O3 powder was dissolved and mixed with ZrO2 during heating, and that many vacancies around the yttrium atoms existed after cooling. A large oxygen deficit around the Y atom and eight O atoms coordinated around Zr may be caused by this metallographic structure.
4.4. Applicability of the developed system to the UO2–Zr reaction
In the present study, we succeeded in simultaneous XAFS–XRD measurements of reaction processes in metals and metal-oxides at ultra-high temperatures above 2000 K. The structural changes in which Zr was oxidized by the impurity oxygen in Ar gas and the ZrO2–Y2O3 reaction proceeded were successfully captured. Since the specimen was very small, it was difficult to measure the temperature using a pyrometer. To solve this problem, temperature calibration was performed using the diffraction pattern of Y2O3, for which there is some knowledge on the temperature dependence of the lattice parameter at high temperatures. Although this method has the limitation that the same equation cannot be used if the heat transfer characteristics of the sample holder change, we think that this method could be applied to different combinations of materials if temperature calibration is performed against the oxide material in advance. Also, in the present study, Zr was oxidized by residual oxygen in the gas phase. To analyze the melting process of UO2–Zr, the oxygen in the furnace must be controlled at a sufficiently low level.
The quality of the obtained spectra was acceptable for 2–Zr mixtures and investigate the structural changes leading to the melting process.
analysis, although the signal-to-noise ratio in the high-energy region tends to deteriorate above ∼2000 K. For diffraction images, it is desirable to be able to scan transmitted X-rays at higher angles to improve the distinguishability of cubic or tetragonal oxide. This can be overcome by improving the equipment, such as widening the glass window at the exit of the chamber's X-ray transmission window. Thus, by implementing some device modifications, it is possible to apply this measurement technique to UO5. Conclusion
In situ simultaneous XAFS–XRD measurements of Y2O3 and Zr–Y2O3 at high temperatures above 2000 K were performed. The signal was taken in transmission mode for the Zr K- and Y K-edges, and the transmitted X-rays were captured by CCD camera as diffraction images. By combining analysis of the XRD patterns and spectra, we succeeded in capturing the structure changes during the Zr oxidation up to 1952 K and the interaction between ZrO2 and Y2O3 for temperatures from 1952 and 2519 K. The interatomic distances obtained by the fitting analysis were confirmed to agree with the literature data for the ZrO2–Y2O3 system. Also, we investigated the temperature dependence of the anharmonic effect by comparing the fitted second- and third-order cumulants, leading to the conclusion that thermal disorder was mainly caused by anharmonic effects during the Y2O3–ZrO2 reaction. Consequently, the developed system in the present study was confirmed to be applicable for investigation of the metal/metal-oxide mixture at extra-high temperature. For application to the melting of material, although some modification on the equipment will be required, it is possible to adapt this technique for investigation of the UO2–Zr reaction leading to the melting process as future work.
Supporting information
Figures S1 to S3. DOI: https://doi.org/10.1107/S1600577524003321/yn5107sup1.pdf
Acknowledgements
The synchrotron radiation experiments were performed at BL22XU of SPring-8 with the approval of the Japan Synchrotron Radiation Research Institute (JASRI) (Proposal Nos. 2023A3710 and 2023B3740).
Funding information
This work was supported by the Innovative Nuclear Research and Development Program by Ministry of Education, Culture, Sports, Science, and Technology (MEXT) in Japan (JPMXD0223813709).
References
Ando, K. & Oishi, Y. (1985). Transport in Nonstoichiometric Compounds, pp. 203–215. Boston: Springer. Google Scholar
Andrievskaya, E. R., Lopato, L. M. & Smirnov, V. P. (1996). J. Am. Ceram. Soc. 79, 714–720. CrossRef CAS Google Scholar
Arroyave, R., Kaufman, L. & Eagar, T. W. (2002). Calphad, 26, 95–118. Web of Science CrossRef CAS Google Scholar
Bessada, C., Zanghi, D., Pauvert, O., Maksoud, L., Gil-Martin, A., Sarou-Kanian, V., Melin, P., Brassamin, S., Nezu, A. & Matsuura, H. (2017). J. Nucl. Mater. 494, 192–199. Web of Science CrossRef CAS Google Scholar
Bessada, C., Zanghi, D., Salanne, M., Gil-Martin, A., Gibilaro, M., Chamelot, P., Massot, L., Nezu, A. & Matsuura, H. (2020). J. Mol. Liq. 307, 112927. Web of Science CrossRef Google Scholar
Boccato, S., Torchio, R., Anzellini, S., Boulard, E., Guyot, F., Irifune, T., Harmand, M., Kantor, I., Miozzi, F., Parisiades, P., Rosa, A. D., Antonangeli, D. & Morard, G. (2020). Sci. Rep. 10, 11663. Web of Science CrossRef PubMed Google Scholar
Butz, B., Kruse, P., Störmer, H., Gerthsen, D., Müller, A., Weber, A. & Iverstiffee, E. (2006). Solid State Ion. 177, 3275–3284. Web of Science CrossRef CAS Google Scholar
Crocombette, J. P. & Jollet, F. (1994). J. Phys. Condens. Matter, 6, 8341–8348. CrossRef CAS Web of Science Google Scholar
Duraud, J., Jollet, F., Thromat, N., Gautier, M., Maire, P., Le Gressus, C. & Dartyge, E. (1990). J. Am. Ceram. Soc. 73, 2467–2473. CrossRef CAS Web of Science Google Scholar
Hayward, P. J. & George, I. M. (1994). J. Nucl. Mater. 208, 35–42. CrossRef CAS Web of Science Google Scholar
Hayward, P. J. & George, I. M. (1996). J. Nucl. Mater. 232, 13–22. CrossRef CAS Web of Science Google Scholar
Hayward, P. J., Hofmann, P., Stuckert, J., Berdyshev, A. V. & Veshchunov, M. S. (1999). UO2 Dissolution by Molten Zircaloy. New Experimental Results and Modelling. Report FZKA-6379. Forschungszentrum Karlsruhe GmbH, Karlsruhe, Germany. Google Scholar
Hofmann, P. & Politis, C. (1979). J. Nucl. Mater. 87, 375–397. CrossRef CAS Web of Science Google Scholar
Jacobson, N. S., Liu, Z. K., Kaufman, L. & Zhang, F. (2004). J. Am. Ceram. Soc. 87, 1559–1566. Web of Science CrossRef CAS Google Scholar
Jonane, I., Lazdins, K., Timoshenko, J., Kuzmin, A., Purans, J., Vladimirov, P., Gräning, T. & Hoffmann, J. (2016). J. Synchrotron Rad. 23, 510–518. Web of Science CrossRef CAS IUCr Journals Google Scholar
Kim, K. T. & Olander, D. R. (1988). J. Nucl. Mater. 154, 102–115. CrossRef CAS Web of Science Google Scholar
Kim, Y.-I. & Izumi, F. (1994). J. Ceram. Soc. Japan, 102, 401–404. CrossRef CAS Google Scholar
Kleykamp, H. (1985). J. Nucl. Mater. 131, 221–246. CrossRef CAS Web of Science Google Scholar
Miyanaga, T. & Fujikawa, T. (1994). J. Phys. Soc. Jpn, 63, 3683–3690. CrossRef CAS Google Scholar
Niino, K., Arita, Y., Konashi, K., Watanabe, H., Yaita, T., Tanida, H., Kobayashi, T., Morimoto, K., Watanabe, M. & Miura, Y. (2023). J. Nucl. Sci. Technol. pp. 1–7. Google Scholar
Okamoto, Y., Osugi, T., Akabori, M., Kobayashi, T. & Shiwaku, H. (2017). J. Mol. Liq. 232, 285–289. Web of Science CrossRef CAS Google Scholar
Ravel, B. & Newville, M. (2005). Phys. Scr. T115, 1007. CrossRef Google Scholar
Rehr, J. J. & Ankudinov, A. L. (2001). J. Synchrotron Rad. 8, 61–65. Web of Science CrossRef CAS IUCr Journals Google Scholar
Seto, Y., Nishio-Hamane, D., Nagai, T. & Sata, N. (2010). Rev. High. Press. Sci. Technol. 20, 269–276. CrossRef Google Scholar
Shirasu, N., Sato, T., Suzuki, A., Nagae, Y. & Kurata, M. (2023). J. Nucl. Sci. Technol. 60, 697–714. Web of Science CrossRef CAS Google Scholar
Shobu, T., Tozawa, K., Shiwaku, H., Konishi, H., Inami, T., Harami, T. & Mizuki, J. (2007). AIP Conf. Proc. 879, 902–906. CrossRef CAS Google Scholar
Skinner, L. B., Benmore, C. J., Weber, J. K. R., Williamson, M. A., Tamalonis, A., Hebden, A., Wiencek, T., Alderman, L. G., Guthrie, M., Leibowitz, L. & Parise, J. B. (2014). Science, 346, 984–987. Web of Science CrossRef CAS PubMed Google Scholar
Skrikanth, V., Sato, A., Yoshimoto, J., Kim, J. H. & Ikegami, T. (1994). Cryst. Res. Technol. 29, 981–984. CrossRef Google Scholar
Swamy, V., Dubrovinskaya, N. A. & Dubrovinsky, L. S. (1999). J. Mater. Res. 14, 456–459. Web of Science CrossRef CAS Google Scholar
Thromat, N., Noguera, C., Gautier, M., Jollet, F. & Duraud, J. P. (1991). Phys. Rev. B, 44, 7904–7911. CrossRef CAS Web of Science Google Scholar
Tim, K. T. & Olander, D. R. (1988). J. Nucl. Mater. 154, 85–101. CrossRef CAS Web of Science Google Scholar
Tuilier, M. H., Dexpert-Ghys, J., Dexpert, H. & Lagarde, P. (1987). J. Solid State Chem. 69, 153–161. CrossRef CAS Web of Science Google Scholar
Xu, Y., Yamazaki, M. & Villars, P. (2011). Jpn. J. Appl. Phys. 50, 11RH02. CrossRef Google Scholar
Yabashi, M., Yamazaki, H., Tamasaku, K., Goto, S., Takeshita, K., Mochizuki, T., Yoneda, Y., Furukawa, Y. & Ishikawa, T. (1999). Proc. SPIE, 3773, 2–13. CrossRef Google Scholar
This is an open-access article distributed under the terms of the Creative Commons Attribution (CC-BY) Licence, which permits unrestricted use, distribution, and reproduction in any medium, provided the original authors and source are cited.