research papers
Synchrotron-radiation X-ray topography of surface strain in large-diameter silicon wafers
aRigaku Corporation, Akishima-shi, Tokyo 196-8666, Japan, bDepartment of Physics, Toyama University, Toyama 930-8555, Japan, cSystem Devices and Fundamental Research, NEC Corporation, Tsukuba 305-8501, Japan, dTOYOTA Central R&D Laboratories Inc., Nagakute-cho, Aichi 480-1192, Japan, eJapan Synchrotron Radiation Research Institute, SPring-8, Mikazuki-cho, Hyogo 679-5198, Japan, fFaculty of Engineering, Kyushu Institute of Technology, Kitakyushu-shi 804-8550, Japan, and gGraduate School of Engineering, Osaka University, Suita, Osaka 565-0871, Japan
*Correspondence e-mail: kawado@rigaku.co.jp
Using a 300 mm-wide monochromatic X-ray beam obtained at beamline BL20B2 of SPring-8, the difference in surface-strain distribution caused by various steps of silicon-wafer manufacturing, i.e. slicing, lapping, etching, grinding and polishing, was studied. The asymmetric 511 reflection of 21.45 keV X-rays, incident at a glancing angle of 0.26°, was used to obtain topographs over the whole surface of a 200 mm-diameter (100) CZ silicon wafer. Differences in crystallinity and in warp between the surfaces at different steps of the manufacturing process (firstly after the lapping following the slicing, and then after successive etching, grinding and polishing) were clearly observed. The former gave a topographic image over the whole area with a one-shot exposure because of their wide rocking curves (50–70 arcsec FWHM), which indicate poor crystallinity. The latter, on the other hand, showed sharper curves (4–5 arcsec FWHM), which indicate good crystallinity in local areas, and the existence of warp, and therefore required step scanning of ω-rotation to cover the whole surface in topography measurements. The effect of each step in the process is also discussed.
Keywords: X-ray topography; asymmetric reflection; silicon wafers; surface strain.
1. Introduction
X-ray diffraction topography has been usefully applied to the characterization of microdefects (Chikawa et al., 1970; Ishikawa, 1989; Iida et al., 1990), growth striations (Kawado et al., 1990; Kudo et al., 1997) and process-induced defects (Tanner, 1976; Boller et al., 1998; Kudo et al., 2001) in silicon. The techniques used in these studies were well sophisticated in most cases. They were, however, unsuitable for practical application, e.g. inspection of as-received silicon wafers used for the LSI fabrication.
Surface-sensitive topography is very useful because semiconductor devices are formed in the surface layers of wafers. Synchrotron plane-wave X-ray topography of 150 mm-diameter silicon wafers was realised at the Photon Factory and revealed growth striations and surface-strain distribution (Kitano et al., 1987).
Recent industrialization of 200 mm- or 300 mm-diameter wafers for ULSI substrates requires more detailed information than ever in crystal imperfections, surface strain, or damage in wafers. For this purpose, development of a large-area X-ray topography technique with high sensitivity to these characteristics is especially desirable.
Recently, we have created an experimental apparatus designed to acquire large-area topographs of silicon crystals at the second experimental hutch of beamline BL20B2 at SPring-8 (Chikaura et al., 2001). This set-up uses the horizontally wide (300 mm) monochromatic X-ray beam realised by the 200 m distance between the hutch and the bending-magnet source point [source size: 0.29 mm (H) × 0.04 mm (V)]. This apparatus, with extremely asymmetric reflections, enabled us to obtain X-ray topographs over the whole surface of a 300 mm-diameter 10 mm-thick silicon crystal with one-shot exposure. In addition, we observed surface damage, e.g. saw marks induced by slicing and minute scratch patterns caused by polishing (Kawado et al., 2000, 2001).
In this paper we report the difference in surface-strain distribution caused by various steps of silicon wafer manufacturing processes, i.e. slicing, lapping, etching, grinding and polishing, in order to optimize the process conditions.
2. Experimental
Wafers were prepared from p-type (B-doped) or n-type (P-doped) 200 mm-diameter CZ silicon crystals with [100] surface orientation and with a resistivity range of 1–10 Ω cm. The crystals were sliced into wafers with a wire saw. The surfaces of the wafers were lapped with #1000-meshed powder, etched with mixed acid and polished mechanically and chemically by the single-sided polish method. This type of polished wafer was designated as A. Wafers of another type, designated as B, were ground with a #3000 whetstone after the etching, and then polished mechanically and chemically. Test samples were picked up at each step of the wafer manufacturing processes. The sample thicknesses are shown in Table 1.
|
A schematic diagram of the experimental arrangement is shown in Fig. 1. A 300 mm-wide X-ray beam monochromated by the Si(311) double-crystal monochromator in the optics hutch was irradiated with skew incidence on the sample wafer in the second experimental hutch. The sample was fixed without glue onto a flat plastic plate attached on a horizontal-axis precision goniometer of tangential-bar type, as is shown in Fig. 2. The energy of the X-ray beam was tuned to be 21.45 keV to use the asymmetric 511 reflection with a glancing angle of 0.26°, which was much larger than the critical angle for total reflection, 0.08°.
Before recording topographs, rocking-curve measurements were carried out in a 2 × 4 mm area on the sample with a ω at fixed 2θB (θB: Bragg angle). Topographs were recorded with a one-shot exposure at the peak position and both wings of the rocking curve for sliced and lapped wafers. On the other hand, step scanning of ω-rotation (angular step of 5 or 10 arcsec) was used for etched, ground and polished wafers since only narrow stripe images were observed in one-shot topographs for these wafers. The topographs were recorded on an imaging plate with a pixel size of 100 × 100 µm, read by an imaging-plate reader and then processed on a personal computer.
by rotating3. Results and discussion
The FWHM (full width at half-maximum) of the rocking curves was useful as a measure of crystallinity although the shape of the rocking curves was influenced by the wavelength spread because of the non-parallel (+n, −m) setting. Table 2 shows the FWHM of the rocking curves measured at the central position of 200 mm-diameter wafers. The FWHM for etched, ground and polished wafers was about one-tenth as small as that for sliced and lapped wafers. Here it should be noted that the grinding resulted in a rather higher degree of crystallinity.
|
To evaluate the thickness of the surface layers characterized by the rocking-curve measurements, the depth of X-ray penetration was calculated on the basis of the ). Since the of the sliced and lapped wafers was regarded as an imperfect crystal, the X-ray penetration was almost equal to the absorption depth, 5.7 µm. On the other hand, the X-ray penetration into the etched, ground and polished wafers was regarded, on account of their high crystallinity, as the extinction distance for the Bragg case in a perfect crystal, 0.9 µm.
of X-ray diffraction (Authier, 2001Figs. 3(a) and 3(b) show two topographs of the sliced and lapped wafers taken at the peak position of the rocking curve. The whole areas of the wafers were observed with one-shot exposure because of the large FWHM. The warp was found, from the difference in the maximum-intensity positions in the topographs taken at both wings of the rocking curve, to be about 200 arcsec and about 80 arcsec for the sliced and lapped wafers, respectively. This result indicates that the lapping caused a considerable reduction in warp by eliminating residual surface damage such as saw marks.
Figs. 4(a) and 4(b) are step-scanned topographs of the etched and ground wafers, showing so-called zebra patterns (Kikuta et al., 1966). The warp was found to be about 55 arcsec and about 290 arcsec for the etched and ground wafers, respectively, by counting the number of stripes and the step interval. The etching resulted in a remarkable improvement in local crystallinity and a reduction in warp, while the grinding after the etching caused a marked increment in warp even though good local crystallinity was maintained, as was indicated by the small FWHM.
Step-scanned topographs of the two polished wafers designated as A and B are shown in Figs. 4(c) and 4(d). The warp was found to be about 150 arcsec and about 170 arcsec for A and B, respectively. Much difference in warp was not found between A and B, although the strain distribution in B was influenced by the grinding from the fact that the zebra pattern in Fig. 4(d) vaguely resembled that in Fig. 4(b). This result means that the grinding is applicable to large-diameter silicon wafer manufacturing processes.
In conclusion, X-ray topography using extremely asymmetric reflection of a 300 mm-wide monochromatic X-ray beam enabled us to obtain some important information about surface-strain distribution caused by the large-diameter silicon wafer manufacturing processes. Clarified effects of the process steps are summarized in Fig. 5.
Acknowledgements
The authors are grateful to Komatsu Electronic Metals Co. Ltd for supplying the test samples. This work was carried out according to the SPring-8 proposal number 2001A0053-ND-np. Technical support of Drs Y. Suzuki, K. Umetani and K. Uesugi at SPring-8 is also appreciated.
References
Authier, A. (2001). Dynamical Theory of X-ray Diffraction, ch. 17. Oxford: Oxford University Press. Google Scholar
Boller, E., Baruchel, J., Pemot, E., Cloetens, P. & Ludwig, W. (1998). ESRF Highlights 1997/1998, pp. 84–85. ESRF, Grenoble, France. Google Scholar
Chikaura, Y., Iida, S., Kawado, S., Mizuno, K., Kimura, S., Matsui, J., Umeno, M., Ozaki, T., Shimura, T., Suzuki, Y., Izumi, K., Kawasaki, K., Kajiwara, K. & Ishikawa, T. (2001). J. Phys. D, 34, A158–162. Web of Science CrossRef CAS Google Scholar
Chikawa, J., Asaeda, Y. & Fujimoto, I. (1970). J. Appl. Phys. 41, 1922–1925. CrossRef CAS Web of Science Google Scholar
Iida, S., Takeno, H., Yagou, Y., Kasagi, N., Sugita, Y. & Kawata, H. (1990). Defect Control in Semiconductors, pp. 1529–1534. Amsterdam: Elsevier. Google Scholar
Ishikawa, T. (1989). Rev. Sci. Instrum. 60, 2490–2493. CrossRef Web of Science Google Scholar
Kawado, S., Iida, S. & Chikaura, Y. (2001). SPring-8 Research Frontiers 1999/2000, pp. 89–91. SPring-8, Hyogo, Japan. Google Scholar
Kawado, S., Iida, S., Ishikawa, K., Chikaura, Y., Suzuki, Y., Kajiwara, K., Kimura, S., Matsui, J., Umeno, M., Shimura, T., Mizuno, K., Ozaki, T., Izumi, K. & Ishikawa, T. (2000). 5th Biennial Conference on High Resolution X-ray Diffraction and Topography (X-TOP 2000). Abstracts, p. 107. Google Scholar
Kawado, S., Kojima, S., Kato, Y., Hayashi, H. & Ishikawa, T. (1990). Defect Control in Semiconductors, pp. 175–180. Amsterdam: Elsevier. Google Scholar
Kikuta, S., Kohra, K. & Sugita, Y. (1966). Jpn. J. Appl. Phys. 5, 1047–1055. CrossRef CAS Web of Science Google Scholar
Kitano, T., Ishikawa, T., Matsui, J., Akimoto, K., Mizuki, J. & Kawase, Y. (1987). Jpn. J. Appl. Phys. 26, L108–110. CrossRef CAS Web of Science Google Scholar
Kudo, Y., Liu, K.-Y., Kojima, S., Kawado, S. & Ishikawa, T. (1997). J. Electrochem. Soc. 144, 4035–4041. CrossRef CAS Web of Science Google Scholar
Kudo, Y., Liu, K.-Y., Kawado, S., Zhang, X. & Hirano, K. (2001). J. Appl. Phys. 90, 670–674. Web of Science CrossRef CAS Google Scholar
Tanner, B. K. (1976). X-ray Diffraction Topography, ch. 4. Oxford: Pergamon Press. Google Scholar
© International Union of Crystallography. Prior permission is not required to reproduce short quotations, tables and figures from this article, provided the original authors and source are cited. For more information, click here.