research papers\(\def\hfill{\hskip 5em}\def\hfil{\hskip 3em}\def\eqno#1{\hfil {#1}}\)

Journal logoJOURNAL OF
APPLIED
CRYSTALLOGRAPHY
ISSN: 1600-5767

Epitaxy of ultrathin Fe3O4 films on SrTiO3(001): influence of growth parameters on the formation of coexisting (111)- and (001)-oriented phases

crossmark logo

aDepartment of Physics, Osnabrück University, Barbarastraße 7, 49076 Osnabrück, Germany, bDeutsches Elektronen-Synchrotron DESY, Notkestraße 85, 22607 Hamburg, Germany, and cSynchrotron SOLEIL, L'Orme des Merisiers, Départementale 128, 91190 Saint-Aubin, France
*Correspondence e-mail: [email protected], [email protected]

Edited by J. Keckes, Montanuniversität Leoben, Austria (Received 19 February 2026; accepted 29 March 2026; online 20 May 2026)

Ultrathin Fe3O4 films were grown on SrTiO3(001) substrates under systematically varied growth conditions (deposition rate and temperature, and film thickness) in order to determine the influence of these parameters on the formation of the coexisting (111) and (001) orientations of Fe3O4. Structural characterization was performed using grazing-incidence X-ray diffraction and high-energy X-ray diffraction, including mapping of the reciprocal space in plane and out of plane to obtain detailed information about the structure of the films in the lateral and vertical directions. Despite an expected cube-on-cube growth, an intermediate layer of (111)-oriented Fe3O4 with hexagonal surface symmetry formed in all samples examined. This intermediate phase occurs in the form of 3D islands during the initial growth phase and persists even after growth has transformed to preferential formation of the (001) orientation. The fraction of the (111) phase, on the other hand, depends heavily on the kinetic conditions during growth. Its formation is favoured by low deposition rates and, above all, high deposition temperatures. These results support earlier observations and provide new insights into the structural development of Fe3O4 films on SrTiO3(001) in the early stages.

1. Introduction

Magnetite (Fe3O4) is of great interest as a candidate for applications in the fields of spintronics (Hoffmann & Bader, 2015View full citation; Hamie et al., 2012View full citation; Seneor et al., 1999View full citation; Kado, 2008View full citation; Wada et al., 2010View full citation; Moussy, 2013View full citation) and spin caloritronics (Ramos et al., 2016View full citation, 2013View full citation; Uchida et al., 2016View full citation) due to a predicted 100% spin polarization at the Fermi level (Zhang & Satpathy, 1991View full citation). However, this promise has not met expectations, which might be due to interface effects (van der Zaag et al., 2000View full citation; Jordan et al., 2006View full citation; Marnitz et al., 2015View full citation; Hu & Suzuki, 2002View full citation; Kado, 2008View full citation). For this reason, detailed knowledge of the growth of ultrathin magnetite films is necessary to control interface and surface properties required for high-quality spintronic devices (Moussy, 2013View full citation; Jordan et al., 2006View full citation).

For the growth of magnetite ultrathin films, various substrates have been used, with MgO(001) being the most widespread. Since its lattice constant results in a small mismatch of Mathematical equation between half the lattice constant of Fe3O4 and MgO, ordered pseudomorphic growth is given (Bertram et al., 2013View full citation, 2012View full citation, 2011View full citation; Wollschläger, 2018View full citation; van der Zaag et al., 2000View full citation; Chang et al., 2016View full citation; Celotto et al., 2003View full citation; Margulies et al., 1997View full citation; Tobin et al., 2007View full citation). However, growth and annealing of Fe3O4 on MgO(001) substrates is limited in temperature, since above 250°C Mg2+ interdiffuses into the magnetite film (Wollschläger, 2018View full citation; Kim-Ngan et al., 2009View full citation).

It has been demonstrated that interdiffusion of ferrite and SrTiO3(001) substrates at elevated temperatures is prohibited (Rodewald et al., 2019View full citation; Thien et al., 2020View full citation). Therefore, despite a large lattice mismatch of Mathematical equation between the SrTiO3 substrate and half the lattice constant of Fe3O4, magnetite films can also be grown on it, even at elevated temperatures (Kuschel et al., 2016View full citation). Furthermore, due to the large lattice mismatch, the use of SrTiO3(001) as a substrate offers the possibility of studying strain effects, which can be used to modify the electronic and magnetic properties of Fe3O4 (Kuschel et al., 2016View full citation; Monti et al., 2013View full citation; Kale et al., 2001View full citation; Rubio-Zuazo et al., 2015View full citation; Liu et al., 2017View full citation; Chen et al., 2008View full citation).

For the growth of Fe3O4 on SrTiO3(001), cube-on-cube growth is expected and is also frequently observed (Kuschel et al., 2017View full citation; Pohlmann et al., 2022View full citation; Alexander et al., 2025View full citation; Wollschläger, 2018View full citation). However, for high temperatures, i.e. T ≥ 700°C, Fe3O4 has been reported to grow in its (111) orientation with hexagonal surface symmetry (Takahashi et al., 2012View full citation, 2014View full citation; Leung et al., 2008View full citation). This effect is attributed to both the large lattice mismatch (7.5%) and the anisotropy of the surface energy of the spinel structure of Fe3O4, which leads to competition between (111) and (001) growth orientations (Mishra & Thomas, 1977View full citation; Yu et al., 2012View full citation; Santos-Carballal et al., 2014View full citation). In recent work, using surface-sensitive spot-profile-analysis low-energy electron diffraction (LEED) measurements, the (111) orientation of Fe3O4 on SrTiO3(001) was observed at even lower temperatures (250°C) as an initial interface structure before it continues to grow in the (001) orien­tation with cubic surface structure (Alexander et al., 2025View full citation).

In this work we analyse the conditions under which the (111) orientation of Fe3O4 is preferentially formed and their influence on the growth behaviour. In particular, the aim is to find out whether the (111) orientation is only a temporary intermediate phase that is transformed into the (001) orientation in the further growth of the thin film or whether this phase persists and coexists with the later (001) orientation.

For this reason, in this work, ultrathin magnetite films have been grown on SrTiO3(001) by reactive molecular beam epitaxy (RMBE) and analysed in situ by means of synchrotron-radiation-based (grazing-incidence) X-ray diffraction (GIXRD) and high-energy X-ray diffraction (HEXRD), providing detailed structural information of the surface, interface and film structure. By varying the growth parameters, their influence on film growth and the formation of the (111) orientation of Fe3O4 was studied.

2. Experimental details

The magnetite thin films were prepared and in situ characterized at the SixS beamline of Synchrotron SOLEIL (Saint-Aubin, France). Here, the diffractometer is coupled to three ultra-high vacuum chambers with a base pressure of 2 × 10−10 mbar, enabling (grazing-incidence) X-ray diffraction experiments directly after film growth without breaking the vacuum (Dawiec et al., 2016View full citation).

Before deposition, the SrTiO3(001) substrates were cleaned by annealing for 90 min at 420°C in a molecular oxygen atmosphere of 5 × 10−5 mbar in order to remove adsorbates.

The films were grown by RMBE, i.e. thermal evaporation from a pure Fe target in a molecular oxygen atmosphere of 5 × 10−6 mbar. During deposition of the first film, the substrate temperature was kept at 420°C and a constant deposition rate was controlled by the flux of the evaporator. This procedure was used to calibrate the deposition rate as recorded by a quartz crystal microbalance prior to the experiments. Afterwards, further samples were prepared by varying one growth parameter at a time, i.e. deposition rate, film thickness and temperature (cf. Fig. 1[link]). Thus, the influence on the growth behaviour of each parameter can be analysed separately.

[Figure 1]
Figure 1
Scheme of studied samples including experimental parameters such as growth temperature, film thickness and deposition rate. First, sample 0 (S0) was analysed as a reference. Subsequently, only one parameter was varied at a time in order to analyse its influence on the structure.

For the following diffraction experiments, a photon energy of 16 keV was used and the data were collected by an XPAD S140 two-dimensional detector. In order to obtain information on the out-of-plane structure of the films, X-ray diffraction (XRD) was performed using the θ–2θ geometry. Subsequently, using a grazing-incidence geometry (GIXRD) with a fixed glancing angle of 0.2°, scans along several crystal truncation rods (CTRs) attributed to Fe3O4(001) and Fe3O4(111) were performed. In the following, the two different Fe3O4 orientations, (001) and (111), are labelled `cub' and `hex', respectively, referring to the square and hexagonal surface structure, respectively. Moreover, two-dimensional in-plane mappings were recorded.

After transport under ambient conditions, films were additionally studied by means of HEXRD at the P07 beamline (EH2) of PETRA III at DESY. For the diffraction experiment, a photon energy of 73.3 keV and a glancing angle of θ = 0.03° were used. The data were collected by a Varex XRD 4343 CT 2D area detector. During the measurement, the samples were rotated between ±90° with a rotation speed of 0.5° s−1 to collect the diffraction signal from the entire sample. Afterwards, the detector images of these scans were summed in order to obtain a full reciprocal-space map of the entire film.

3. Results

3.1. Reference sample S0

Fig. 2[link] shows an in-plane reciprocal-space map for low L values {0.02 < L < 0.1 [r.l.u. (reciprocal-lattice units) SrTiO3(001)]}. Besides the expected reflections of the SrTiO3 substrate (green crosses) and reflections of the cubic (001) orientation of Fe3O4 (red squares), reflections with a 12-fold symmetry can be found. These are reflections of the hexagonal surface structure of Fe3O4(111), which is present in two domains, A (yellow circles) and B (yellow diamonds), rotated by 90°, as well as the respective mirror domains Mathematical equation and Mathematical equation. The latter two domains are not found in Fig. 2[link] as their in-plane reflections fully overlap with reflections from A and B. However, the mirror domains can be distinguished using higher out-of-plane scattering vectors (higher values of L).

[Figure 2]
Figure 2
Section of an in-plane reciprocal-space map of reference sample for summation of intensities running the scaled out-of-plane scattering-vector magnitude L between 0.02 and 0.1 [r.l.u. SrTiO3(001)]. For reasons of clarity, only reflections/CTRs that can be detected are included.

Since Mathematical equation coincides with (220)cub [close to (110)STO], it is evident that the orientation of Fe3O4(111) with respect to the substrate is

Mathematical equation

and

Mathematical equation

and analogously for their mirror domains Mathematical equation and Mathematical equation, respectively. A graphical representation of the orientation of Fe3O4(111) on the substrate is shown in Fig. 3[link]. The 12-fold symmetry and the positions of the in-plane Fe3O4(111) reflections show that the Fe3O4(111) layer is (almost) fully relaxed. This result contradicts the model proposed by Takahashi et al. (2012View full citation), which suggests that the Fe3O4(111) film adapts to the lattice of the SrTiO3(001) substrate in the sense of a superstructure. This would lead to distorted diffraction patterns with a sixfold instead of a 12-fold symmetry.

[Figure 3]
Figure 3
Schematic model for the in-plane orientation of Fe3O4(111) grown on SrTiO3(001). The larger green circles denote the Sr2+ cations and the smaller red circles represent the Fe3+ cations of the Fe3O4(111) unit cell. For simplicity, Ti and O atoms are not shown and the surface unit cell of Fe3O4(111) is used. The two possible domains, A and B, rotated by 90°, are shown. [Adapted from Leung et al. (2008View full citation).]

The cross-shaped weak intensities around the Fe3O4(001) reflections indicate facets with an in-plane component in the 〈110〉 directions.

Since only the square surface structure of the Fe3O4(001) can be seen with surface-sensitive electron diffraction (LEED), here it can be concluded from the presence of the Fe3O4(111) reflections that the (111) orientation is not a temporary intermediate phase that transforms into the (001). Rather, a permanent Fe3O4(111) interlayer is stabilized at the interface that continues to coexist with the Fe3O4(001) film.

Fig. 4[link](a) presents a (00L) XRD scan performed at the reference sample. Besides the expected reflections of the substrate, the (004)cub reflection can be seen due to (001)-oriented (majority) fractions of the Fe3O4 film. Near this Bragg peak, no Laue fringes are observed, pointing to an inhomogeneous crystalline order of Fe3O4(001).

[Figure 4]
Figure 4
(a) XRD scan along the (00)-CTR of the reference sample. Since nothing can be seen in the range L < 1.5 except for the substrate reflection, this is not shown. (b) L scan along the Mathematical equation-CTR of Fe3O4(001) of the reference sample (HK ≈ 0.93, cf. Fig. 2[link]). Here, the sharp outliers at L = 1 and L = 2 are due to diffuse scattering close to very intense substrate Bragg peaks being close to the measured Fe3O4 CTR. (c) Schematic sketch of the reflections expected on and near the Mathematical equation-CTR of completely relaxed Fe3O4(001) and Fe3O4(111).

Furthermore, the (222)hex reflection, expected at L = 1.62, is not present. Although the intensity of Fe3O4(222) is weak compared with Fe3O4(004) due to its structure factor, the complete absence of the reflection indicates that most of the Fe3O4 film grows with the (001) orientation.

The full width at half-maximum (FWHM) of (004)cub is used to determine the crystalline film thickness dcryst according to the Scherrer formula (Scherrer, 1918View full citation):

Mathematical equation

with KS = 0.89 and af being the bulk lattice constant of Fe3O4. This results in a crystalline film thickness dcryst = 14.0 (2) nm. A comparison with the deposited film thickness shows that dcryst is only slightly lower, meaning that most of the layer is ordered crystalline.

Fig. 4[link](b) shows the diffractogram recorded for the Mathematical equation-CTR of Fe3O4(001). Fe3O4 reflections due to both Fe3O4(001) and Fe3O4(111) can lie on this CTR [cf. Fig. 4[link](c)]. Besides the two Fe3O4-related reflections (222)cub and (224)cub at L = 0.93 and L = 1.86, respectively, an additional reflection is present at L = 0.81. This reflection is attributed to Mathematical equation of Fe3O4(111).

The intensities of (222)cub and Mathematical equation are used to determine the quantity of (111)-orientated Fe3O4. For this, the structure factors FHKL of the respective reflections must be taken into account. Structure factors were calculated from the spinel structure using atomic form factors from Brown et al. (2006View full citation). Consequently, the normalized intensity yield Yhex/cub, i.e. the fraction of Fe3O4 with (111) orientation, can be calculated as

Mathematical equation

Only the Fe3O4(111) reflections of one domain and its mirror domain (here, A and Mathematical equation) are apparent at this position. Assuming a statistically uniform distribution of the domains, the overall fraction of Fe3O4 with (111) orientation is twice as high, i.e. Mathematical equation.

Taking this result and the respective structure factors into account, it is obvious that the (222)hex reflection, which would be expected at approximately L = 1.62 on the (00L) CTR, is not visible in the XRD measurement [cf. Fig. 4[link](a)], as its intensity is only Mathematical equation of that of (004)cub and it therefore vanishes into the background. The same applies to (111)hex, expected at L = 0.81.

From the vertical difference between the two reflections (222)cub and (224)cub, a vertical lattice constant of a = 839.2 (10) pm can be determined. Within the experimental uncertainty, this is in good agreement with the value of 839.6 pm for bulk magnetite (Cornell & Schwertmann, 2003View full citation), demonstrating again complete relaxation of the Fe3O4(001) film in the vertical direction. A detailed discussion will be presented later.

The FWHM analysis of the reflections shows that for Fe3O4(001) there is a broadening of the FWHM with increasing scattering-vector magnitude q, which is nearly linear (cf. Fig. 5[link]). This broadening with increasing scattering vector indicates mosaics, i.e. parts of the surface that are slightly tilted with respect to the SrTiO3(001) surface. In this case, the broadening of the spot profiles is related to the spread of the tilted mosaics, i.e. the sharpness of the distribution of mosaic angles, which is highly dependent on the lattice mismatch (Wollschläger et al., 2001View full citation). The slope of the linear incline corresponds to the mosaic spread Δσ, while the FWHM for the extrapolation Mathematical equation is caused by finite size effects resulting from the size of the mosaics. These mosaics can be attributed to the formation of misfit dislocations at the interface for strain release caused by the lattice mismatch between Fe3O4(001) and SrTiO3(001) as observed in different material systems with high lattice mismatch (Goldbach & Wollschläger, 2022View full citation; Wollschläger et al., 2001View full citation; Dynna et al., 1996View full citation; Vassent et al., 1996View full citation). Since the broadening of the reflections is perpendicular to the origin or to the scattering vector q but the L scan only measures the vertical component of the FWHM, a corresponding correction must be made for each measured FWHM in order to calculate the projection of the FWHM (cf. inset in Fig. 5[link]).

[Figure 5]
Figure 5
FWHM analysis of (LLL) reflections of (001)-oriented Fe3O4 of the reference sample as a function of the scattering-vector magnitude q. The FWHM of the peaks has been fitted with a linear function. The inset shows the projection of the effective FWHM onto the measured vertical FWHM.

A fitting of the FWHM with a linear function (cf. Fig. 5[link]) results in a mosaic spread of Δσ = 1.82 (4)° and a constant offset of 0.066 (r.l.u. Fe3O4) that corresponds to a lateral mosaic size of dmosaic = 11.3 (2) nm with respect to the [111] direction.

3.2. Influence of deposition rate

The first variation in film growth parameters was a higher deposition rate, achieved by increasing the material flux of the evaporator. Therefore, the deposition rate was increased from 0.375 to 0.750 nm min−1 while keeping the deposition temperature and final film thickness constant. For the latter, the deposition time was halved.

Qualitatively, no significant difference can be seen in the in-plane maps with a change in the deposition rate (cf. Fig. 6[link]). The reflections of the (111) orientation (white arrows) are slightly more pronounced at a lower deposition rate, especially the non-integer CTRs without in-plane reflections (red arrows). In addition, the crosses caused by facets on the Fe3O4(001) reflections are slightly more pronounced, which indicates that the proportion of facets has increased, i.e. larger facets have been formed or more facets have been formed.

[Figure 6]
Figure 6
Comparison of the in-plane reciprocal-space maps of the reference sample (left) and the sample with higher deposition rate (right). The L value is a summation between 0.02 and 0.1 [r.l.u. SrTiO3(001)] (cf. Fig. 2[link]). The white arrows denote in-plane reflections of the (111) orientation, while the red arrows denote CTRs of the (111) orientation without in-plane reflections.

In the XRD measurements on the (00L) rod with a higher deposition rate, there is also no significant difference from the reference sample [cf. Fig. 7[link](a)]. The (004)cub reflection has a slightly higher intensity, so that it is more apparent.

[Figure 7]
Figure 7
(a) Comparison of XRD scans along the (00)-CTR for different deposition rates. (b) Comparison of L scans along the Mathematical equation-CTR of Fe3O4(001) for different deposition rates. Here, the sharp outliers at L = 1 and L = 2 are due to diffuse scattering close to very intense substrate Bragg peaks being close to the measured CTRs.

The FWHM of (004)cub gives a crystalline layer thickness of dcryst = 12.9 (2) nm according to equation (1[link]). Despite the initial deposited volume of Fe3O4 being the same, this is slightly lower than for the reference sample, which could be explained by the fact that the layer with the lower growth rate can arrange its structure better.

Equally on the (22)cub-CTR, no significant qualitative difference can be seen between the two samples [cf. Fig. 7[link](b)]. The reflection Mathematical equation belonging to the (111) orientation of Fe3O4 can also be seen for both preparations. Using the intensity ratio of (222)cub and Mathematical equation according to equation (2[link]), the fraction of (111)-orientated Fe3O4 (both A and Mathematical equation domains) in the sample with the higher deposition rate is Mathematical equation. This is a decrease by half compared with the reference sample, suggesting that a lower deposition rate favours the formation of the (111) orientation, and supports the qualitative observations from the comparison of the in-plane maps for the two preparations (cf. Fig. 6[link]).

Fig. 8[link] shows the FWHM versus the scattering-vector magnitude q for the Fe3O4(001) reflections. The sample with a higher deposition rate also shows a widening with q, which indicates tilting mosaics. For this reason, the FWHM was fitted with a linear function to determine the mosaic size dmosaic and the mosaic spread Δσ. Similarly to the crystalline film thickness, the lateral mosaic size with respect to the [111] direction for the sample with a higher deposition rate is slightly lower at dmosaic = 10.3 (2) nm than for the reference sample [dmosaic = 11.3 (2) nm].

[Figure 8]
Figure 8
FWHM analysis of (LLL) reflections of (001)-oriented Fe3O4 as a function of the scattering-vector magnitude q for different deposition rates. The FWHM of the peaks has been fitted with a linear function.

From the slope of the FWHM with q, a mosaic spread of Δσ = 1.34 (4)° is obtained for the sample with a higher deposition rate. This is also slightly lower than that for the reference sample [Δσ = 1.82 (4)°], which indicates a sharper distribution of mosaic angles with a higher deposition rate.

3.3. Influence of film thickness

The second variation in film growth parameters was a lower film thickness df. To achieve this, the deposition time was reduced to one-third of that used for the reference sample while the deposition rate and temperature were kept constant.

Because there was insufficient signal intensity from the magnetite film, no in-plane map could be recorded, while it was possible to record out-of-plane scans.

There are no significant qualitative differences either in the XRD measurement along the (00)-CTR or in the L scan along the (22)cub-CTR (cf. Fig. 9[link]). The intensity of the reflections is evidently weaker in the thinner film, as expected due to the probed film volume. Since (004)cub could not be reasonably fitted due to its low intensity, it was not possible to determine the crystalline layer thickness according to the Scherrer equation.

[Figure 9]
Figure 9
(a) Comparison of XRD scans along the (00)-CTR for films of different thicknesses. (b) Comparison of L scans along the Mathematical equation-CTR of Fe3O4(001) for different film thickness. Here, the sharp outliers at L = 1 and L = 2 are due to diffuse scattering close to very intense substrate Bragg peaks being close to the measured CTRs.

The intensity ratio between Mathematical equation and (222)cub as obtained from the (22)cub-CTR of Fe3O4(001) results in a fraction of (111)-oriented Fe3O4 of Mathematical equation according to equation (2[link]). Compared with the reference sample, this is an increase in the proportion by a factor of 2.5 and corresponds very well to the respective reduction in film thickness. This means that the (111) orientation forms directly at the beginning of film growth and the Fe3O4 film then continues to grow exclusively in the (001) orientation. The (111) orientation is therefore present as a permanent intermediate layer.

The reflections of Fe3O4(001) also broaden with increasing q for the sample with a lower layer thickness (cf. Fig. 10[link]). The fit gives a lateral mosaic size with respect to the [111] direction of dmosaic = 5.0 (2) nm and a mosaic spread of Δσ = 1.36 (4)°. Since the crystalline layer thickness dcryst could not be determined using the XRD scan along the (00L) rod, the projection of the mosaic size perpendicular to the substrate [Mathematical equation] is used to estimate the crystalline film thickness. Accordingly, the crystalline layer thickness dcryst must be in-between the vertical mosaic size Mathematical equation and the evaporated film thickness df, i.e. 4.0 < dcryst < 5.6 nm.

[Figure 10]
Figure 10
FWHM analysis of (LLL) reflections of (001)-oriented Fe3O4 as a function of the scattering-vector magnitude q for different film thicknesses. The FWHM of the peaks has been fitted with a linear function.

The mosaic spread is lower than for the reference sample and indicates that the distribution of mosaic angles is sharper at the beginning of the growth and broadens with increasing film thickness.

3.4. Influence of deposition temperature

The third variation in film growth parameters was a higher deposition temperature. The deposition temperature was increased from 420 to 700°C, while the deposition rate and time (film thickness) were kept constant.

Fig. 11[link] shows the comparison of the reciprocal in-plane maps for deposition at different temperatures. All reflections of Fe3O4, from both (001) and (111) orientations, are significantly sharper and more pronounced in the sample that was grown at a higher temperature. This indicates higher crystalline order in the lateral direction for both orientations of Fe3O4. Furthermore, the cross-shaped weak intensities around the Fe3O4(001) reflections caused by facets can be seen here. Although these are sharper, they are less pronounced compared with those for the film deposited at lower temperature (reference sample).

[Figure 11]
Figure 11
Comparison of the in-plane reciprocal-space maps of the reference sample (left, deposition temperature 420°C) and the sample with increased deposition temperature (right, 700°C). The L value is a summation between 0.02 and 0.1 [r.l.u. SrTiO3(001)]. The dark regions on the right-hand side are artefacts caused by the overlap of the individual detector images.

In the XRD scan along the (00L) rod [cf. Fig. 12[link](a)], the reflections of the (001) orientation of Fe3O4 are sharp and clearly pronounced, which indicates a high crystalline order. Furthermore, at L = 0.81 and L = 1.62, the two reflections of the (111) orientation, (111)hex and (222)hex, respectively, are clearly recognisable. Accordingly, Fe3O4 is present in its (111) orientation in a significant proportion. The L scan along the (22)cub-CTR of Fe3O4(001) also provides a comparable result [see Fig. 12[link](b)]. Here, too, all Fe3O4 reflections are sharper and more pronounced than for diffraction reflections obtained from the film deposited at lower temperature, especially Mathematical equation belonging to the (111) orientation. The intensity ratio according to equation (2[link]) results in a proportion of Mathematical equation for (111)-orientated Fe3O4. Compared with the reference sample, this is a significant increase in the proportion of (111) orientation by a factor of 12.6 and confirms previous work that higher temperatures favour the (111) orientation of Fe3O4 on SrTiO3(001) (Takahashi et al., 2012View full citation, 2014View full citation; Leung et al., 2008View full citation).

[Figure 12]
Figure 12
(a) Comparison of XRD scans along the (00)-CTR for different deposition temperatures. (b) Comparison of L scans along the Mathematical equation-CTR of Fe3O4(001) for different deposition temperatures. Here, the sharp outliers at L = 1 and L = 2 are due to diffuse scattering close to very intense substrate Bragg peaks being close to the measured CTRs.

The FWHM of (004)cub results in a crystalline film thickness of dcryst = 16.0 (2) nm, which is in very good agreement with the deposited amount of Fe3O4 and is the highest value among the samples studied. This is probably due to the increased growth kinetics, which favour a better ordering of the layer. Since reflections of the (111) orientation of Fe3O4 can be seen in this sample on the (00L) rod, these can also be used to determine the crystalline film thickness of the (111) orientation according to Scherrer [equation (1[link])]. This results in a crystalline film thickness of dcryst = 9.3 (2) nm. Since both orientations of Fe3O4 together far exceed the amount of Fe3O4 deposited, the (111) orientation cannot be a continuous laminar intermediate layer. Rather, the (111)-oriented Fe3O4 must be present in the form of 3D islands, covered by the (001)-oriented Fe3O4 (cf. Fig. 13[link]). In addition, the space between (111)-oriented 3D islands is filled by the (001)-oriented Fe3O4 film.

[Figure 13]
Figure 13
Schematic sketch of the grown film. The initial (111)-oriented Fe3O4 grows in 3D islands on the SrTiO3(001) substrate. Afterwards, the space between these islands is filled and covered by (001)-oriented Fe3O4. Even though, for reasons of simplicity, the (111) orientation has been sketched here as simple islands on the substrate, it cannot be excluded that an additional thin layer of (111)-oriented Fe3O4 exists at the interface, meaning that this is a case of layer-plus-island growth (Stranski–Krastanov). This structure applies generally to all samples studied. Only the respective layer thicknesses and the proportion of (111) islands differ.

A comparable result can also be observed in the other samples. However, since the samples do not show any reflections of the (111) orientation on the (00)-CTR, Mathematical equation must be used for this analysis. Since additional broadening due to mosaics cannot be excluded, only the minimum crystalline thickness that the (111) orientation must have can be estimated. Nevertheless, the minimum thickness for all samples is significantly higher than what would be expected for a laminar layer structure, i.e. yield × deposited thickness, so that the island model is also applicable to the other samples.

In the same way as with the other samples, there is also a broadening of the Fe3O4(001) reflections with q in the sample that was grown at a higher temperature (cf. Fig. 14[link]). A fit here results in a lateral mosaic size with respect to the [111] direction of dmosaic = 12.1 (2) nm and a mosaic spread of Δσ = 0.93 (4)°. The mosaic spread is the lowest of all four samples, which means that the mosaics are more ordered and tend to have a preferred direction, as well as the largest lateral extension.

[Figure 14]
Figure 14
FWHM analysis of (LLL) reflections of (001)-oriented Fe3O4 as a function of the scattering-vector magnitude q for different deposition temperatures. The FWHM of the peaks has been fitted with a linear function. As the data point on the (111)cub-CTR deviates significantly from the trend of the other data, it was not considered in the fit.

3.5. HEXRD

To gain a deeper insight into the complete in-plane and out-of-plane structure of the ultrathin films, the samples were analysed a posteriori using HEXRD. Fig. 15[link] shows a section of the reciprocal-space map for the samples analysed near the (22)cub- and (11)STO-CTRs, where reflections are expected from both the (001) and (111) orientations of Fe3O4.

[Figure 15]
Figure 15
Sections of the recorded HEXRD reciprocal-space map for all four samples. The dark rectangles at the positions of the SrTiO3 reflections are caused by beamstops used to protect the detector from the substrate's bright Bragg reflections.

As with the GIXRD in-plane map, only the more intense reflections are visible in the thin sample, even from the (001) orientation. In addition to the reflections of the Fe3O4(001) orientation, Mathematical equation on the (22)cub-CTR can be seen in the reference sample and the high-rate sample. In the high-temperature sample, on the other hand, all the expected reflections from the (111) orientation can be seen, except for the one that would be expected at approximately Mathematical equation [r.l.u. SrTiO3(001)]. However, this is Mathematical equation, which is significantly weaker than the other reflections due to the low form factor [cf. the (133)cub reflection to its left, which is barely visible even at the (001) orientation]. It is noticeable that the (111) orientation in the reference sample and the high-rate sample is slightly laterally distorted or not fully relaxed, as Mathematical equation is not fully aligned with the (22)cub-CTR, as expected for relaxed Fe3O4(001), but is slightly shifted towards the substrate reflection. This is not the case with the high-temperature sample, where the film is (almost) completely relaxed.

Analogously to the GIXRD in-plane map (cf. Section 3.1[link]), the positions of the Fe3O4(111) reflections contradict the model proposed by Takahashi et al. (2012View full citation). Even though, in the case of the reference sample and the high-rate sample, the (111) orientation is not laterally relaxed, suggesting an initial adaptation to the SrTiO3(001) substrate's lattice, the lateral lattice vectors of the structure proposed by the Takahashi model would result in an expansion of Mathematical equation in the Mathematical equation direction and a compression of Mathematical equation in the [410] direction. Due to the projection of all lateral scattering vector components q|| over a larger angle range of ±90°, this would be apparent in the HEXRD out-of-plane reciprocal-space map as a double reflection at the position of Mathematical equation, which is not the case in the present measurements.

To obtain information about the vertical and lateral lattice constants a and a|| for the possibly tetragonally distorted Fe3O4(001) film, the positions in reciprocal space of the visible reflections of the film were determined. Up to 15 Bragg peaks per sample were fitted with 2D Gaussians to obtain both their out-of-plane and their in-plane positions. If these positions in reciprocal lattice units of SrTiO3 are then plotted against their nominal positions in lattice units of Fe3O4 and fitted with a linear function, the slope of this function corresponds to the ratio of the lattice constants between the substrate and the film [cf. Fig. 16[link](a)].

[Figure 16]
Figure 16
(a) Determination of the vertical (blue) and lateral (red) lattice constants for the high-temperature sample. By plotting the fitted reflection positions against their nominal positions, the ratio of the lattice constants of the film and substrate can be obtained from the slope (dashed line). (b) Lateral and vertical lattice constants a|| and a versus the crystalline layer thickness dcryst of Fe3O4(001) determined from the fit in the HEXRD measurements. For comparison, the vertical lattice constants a determined from the difference of the reflections on the (22)cub-CTR are also plotted. The black dashed line denotes the value for bulk Fe3O4.

Fig. 16[link](b) shows the vertical and lateral lattice constants determined in the above method for the (001) orientation of Fe3O4, as well as the vertical lattice constant determined from the difference between the (222)cub and (224)cub reflections (cf. Section 3.1[link]). The values for the vertical lattice constants determined using different methods agree very well within the range of errors, confirming the validity of both approaches. Within the limits of accuracy, all films except the thickest (high-temperature sample) are tetragonally distorted because their in-plane and out-of-plane lattice constants are different. For the vertical lattice constant, it can be seen that this increases with the crystalline film thickness dcryst and approaches the value of bulk Fe3O4. This means that vertical compression is initially present and the film gradually relaxes as the thickness increases. Note that (except for the reference sample and the low-thickness sample) other parameters (rate, temperature) were also changed for each film thickness. For dcryst > 11.9 (2) nm, the Fe3O4(001) film is fully relaxed in its vertical direction.

In the lateral direction, however, the film is initially expanded and relaxes (excluding the lower-thickness sample) as the film thickness increases, so that it is completely relaxed in the lateral direction as well for dcryst > 14.0 (2) nm. How­ever, since the doubled lattice constant of SrTiO3(001) (Mathematical equation) is Mathematical equation smaller than that of Fe3O4(001), lateral compression and vertical expansion are to be expected for pseudomorphic growth of ultrathin films and taking into account the theory of elastic strain. Nevertheless, this unusual strain with lateral expansion and vertical compression has already been observed in previous studies on thin films of Fe3O4, NiFe2O4 and CoFe2O4 on SrTiO3(001), but so far there is no explanation for this behaviour (Gao et al., 2009View full citation; Hoppe et al., 2015View full citation; Moyer et al., 2012View full citation; Thien et al., 2020View full citation; Rodewald et al., 2020View full citation; Kuschel et al., 2017View full citation).

To determine the vertical and lateral layer distances c and c|| of the (111) orientation, Mathematical equation was used, as it was the only reflection that could be fitted for all samples except for that with lower thickness (cf. Table 1[link]). Here, the vertical and lateral layer distances c and c|| denote the layer distance of the (111) orientation of Fe3O4 in the [111] and Mathematical equation directions, respectively. For bulk Fe3O4, c = 484.7 pm and c|| = 296.8 pm (Cornell & Schwertmann, 2003View full citation). Besides the high-temperature sample, the vertical layer distances determined from the HEXRD measurements and from the reflection position on the (22)cub-CTR (GIXRD experiment) differ significantly from each other. This could be because, contrary to the assumption made in the GIXRD reciprocal-space maps (cf. Fig. 2[link]), the (001) and (111) orientations fully overlap; in the reference sample and the high-rate sample Mathematical equation does not coincide exactly with the (22)cub-CTR (cf. Fig. 15[link]). Due to its tilted orientation, its position in the L scan for the GIXRD experiment is overestimated (cf. Fig. 17[link]).

Table 1
Lateral and vertical layer distances c|| and c of the (111) orientation of Fe3O4 determined from the fit in the HEXRD measurements

For comparison, the vertical layer distances c determined from the measurement of the (22)cub-CTR are also plotted. The layer distances of the low-thickness sample could not be determined due to the absence of the Mathematical equation reflection.

  Mathematical equation (pm) Mathematical equation (pm) Mathematical equation (pm)
Reference sample 294.2 (7) 499.5 (12) 488.0 (5)
Higher rate 295.9 (7) 495.8 (12) 485.0 (5)
Higher temperature 297.8 (7) 480.4 (12) 481.0 (5)
[Figure 17]
Figure 17
Schematic representation of how the position of a reflection located slightly outside the region of interest (ROI) is misinterpreted.

In all three cases, the (111)-oriented films are highly strained compared with bulk Fe3O4 (c = 484.7 pm and c|| = 296.8 pm). However, while the reference sample and high-rate sample are vertically expanded and laterally compressed, the high-temperature sample exhibits vertical compression and lateral expansion.

4. Summary

Ultrathin Fe3O4 films were grown on SrTiO3(001) substrates under various growth conditions to investigate the influence of these parameters on the formation of the (111) orientation of Fe3O4. These films were then studied using in situ GIXRD and ex situ HEXRD, and both in-plane and out-of-plane reciprocal-space maps were recorded to obtain detailed structural information in both the lateral and vertical directions.

All samples grown exhibit high crystallinity, with the growth conditions and thus the kinetic parameters being crucial for the resulting structure. The lattice constants determined show a dependence on dcryst (and other variations of the parameters for film preparation) and an atypical strain that cannot be explained by the standard theory of epitaxy. Moreover, all samples show mosaicity, which indicates misfit dislocations due to the high lattice mismatch between the film and substrate. The main structural changes are summarized in Fig. 18[link].

[Figure 18]
Figure 18
Schematic summary of the main structural changes in the samples studied by changing the growth parameters.

In addition to the expected (001) orientation of Fe3O4, the (111) orientation is present in all samples studied, forming four rotational domains. The formation of the (111) orientation is favoured by low deposition rates and, in particular, increased deposition temperatures. Investigations on the low-thickness sample show that the (111)-oriented film is predominantly formed at the beginning of film growth and then persists and coexists with the later formed (001) orientation. This (111) orientation forms 3D islands that are subsequently covered or filled by Fe3O4 with (001) orientation, which confirms previous investigations (Alexander et al., 2025View full citation).

Acknowledgements

We acknowledge SOLEIL (Saint-Aubin, France) for the provision of beam time within the standard proposal 20191762 and we thank the synchrotron staff for assistance in using beamline SixS. We thank DESY (Hamburg, Germany), a member of the Helmholtz Association HGF, for the provision of experimental facilities. Parts of this research were carried out at PETRA III beamline P07 EH2. Beam time was allocated for proposal I-20230571. Furthermore, we acknowledge support by the PETRA III sample environment group. Open access funding enabled and organized by Projekt DEAL.

Funding information

Financial support from the Deutsche Forschungsgemeinschaft (DFG under Nos. KU2321/6-1, KU2321/6-2 and WO533/20-1) is gratefully acknowledged.

References

Return to citationAlexander, A., Kleideiter, T., Pollenske, T., Ruwisch, K., Bertram, F. & Wollschläger, J. (2025). Appl. Surf. Sci. 684, 161835.  CrossRef Google Scholar
Return to citationBertram, F., Deiter, C., Hoefert, O., Schemme, T., Timmer, F., Suendorf, M., Zimmermann, B. & Wollschläger, J. (2012). J. Phys. D Appl. Phys. 45, 395302.  Web of Science CrossRef Google Scholar
Return to citationBertram, F., Deiter, C., Pflaum, K., Suendorf, M., Otte, C. & Wollschläger, J. (2011). J. Appl. Phys. 110, 102208.  Web of Science CrossRef Google Scholar
Return to citationBertram, F., Deiter, C., Schemme, T., Jentsch, S. & Wollschläger, J. (2013). J. Appl. Phys. 113, 184103.   Google Scholar
Return to citationBrown, P. J., Fox, A. G., Maslen, E. N., O'Keefe, M. A. & Willis, B. T. M. (2006). International Tables for Crystallography, Vol. C, Mathematical, Physical and Chemical Tables, edited by E. Prince, ch. 6.1, pp. 554–595. International Union of Crystallography.  Google Scholar
Return to citationCelotto, S., Eerenstein, W. & Hibma, T. (2003). Eur. Phys. J. B Condens. Matter 36, 271–279.  CAS Google Scholar
Return to citationChang, C., Hu, Z., Klein, S., Liu, X., Sutarto, R., Tanaka, A., Cezar, J., Brookes, N., Lin, H.-J., Hsieh, H., Chen, C., Rata, A. & Tjeng, L. (2016). Phys. Rev. X 6, 041011.  Google Scholar
Return to citationChen, Y. Z., Sun, J. R., Han, Y. N., Xie, X. Y., Shen, J., Rong, C. B., He, S. L. & Shen, B. G. (2008). J. Appl. Phys. 103, 07D703.   Google Scholar
Return to citationCornell, R. M. & Schwertmann, U. (2003). The Iron Oxides: Structure, Properties, Reactions, Occurences and Uses. Wiley-VCH Verlag.  Google Scholar
Return to citationDawiec, A., Garreau, Y., Bisou, J., Hustache, S., Kanoute, B., Picca, F., Renaud, G. & Coati, A. (2016). J. Instrum. 11, P12018–P12018.  Google Scholar
Return to citationDynna, M., Vassent, J. L., Marty, A. & Gilles, B. (1996). J. Appl. Phys. 80, 2650–2657.  CrossRef CAS Google Scholar
Return to citationGao, X. S., Bao, D. H., Birajdar, B., Habisreuther, T., Mattheis, R., Schubert, M. A., Alexe, M. & Hesse, D. (2009). J. Phys. D Appl. Phys. 42, 175006.  Web of Science CrossRef Google Scholar
Return to citationGoldbach, H. D. & Wollschläger, J. (2022). J. Vac. Sci. Technol. A 40, 033403.   Google Scholar
Return to citationHamie, A., Dumont, Y., Popova, E., Fouchet, A., Warot-Fonrose, B., Gatel, C., Chikoidze, E., Scola, J., Berini, B. & Keller, N. (2012). Thin Solid Films 525, 115–120.  CrossRef CAS Google Scholar
Return to citationHoffmann, A. & Bader, S. D. (2015). Phys. Rev. Appl. 4, 047001.   Google Scholar
Return to citationHoppe, M., Döring, S., Gorgoi, M., Cramm, S. & Müller, M. (2015). Phys. Rev. B 91, 054418.  CrossRef Google Scholar
Return to citationHu, G. & Suzuki, Y. (2002). Phys. Rev. Lett. 89, 276601.  CrossRef PubMed Google Scholar
Return to citationJordan, K., Cazacu, A., Manai, G., Ceballos, S. F., Murphy, S. & Shvets, I. V. (2006). Phys. Rev. B 74, 085416.  CrossRef Google Scholar
Return to citationKado, T. (2008). Appl. Phys. Lett. 92, 092502.   Google Scholar
Return to citationKale, S., Bhagat, S. M., Lofland, S. E., Scabarozi, T., Ogale, S. B., Orozco, A., Shinde, S. R., Venkatesan, T., Hannoyer, B., Mercey, B. & Prellier, W. (2001). Phys. Rev. B 64, 205413.  CrossRef Google Scholar
Return to citationKim-Ngan, N.-T., Balogh, A., Meyer, J., Brötz, J., Zając, M., Ślęzak, T. & Korecki, J. (2009). Surf. Sci. 603, 1175–1181.  CAS Google Scholar
Return to citationKuschel, O., Buß, R., Spiess, W., Schemme, T., Wöllermann, J., Balinski, K., N'Diaye, A. T., Kuschel, T., Wollschläger, J. & Kuepper, K. (2016). Phys. Rev. B 94, 094423.  CrossRef Google Scholar
Return to citationKuschel, O., Spiess, W., Schemme, T., Rubio-Zuazo, J., Kuepper, K. & Wollschläger, J. (2017). Appl. Phys. Lett. 111, 041902.  Web of Science CrossRef Google Scholar
Return to citationLeung, G. W., Vickers, M. E., Yu, R. & Blamire, M. G. (2008). J. Cryst. Growth 310, 5282–5286.  CrossRef CAS Google Scholar
Return to citationLiu, X. H., Liu, W. & Zhang, Z. D. (2017). Phys. Rev. B 96, 094405.  CrossRef Google Scholar
Return to citationMargulies, D. T., Parker, F. T., Rudee, M. L., Spada, F. E., Chapman, J. N., Aitchison, P. R. & Berkowitz, A. E. (1997). Phys. Rev. Lett. 79, 5162–5165.  Web of Science CrossRef CAS Google Scholar
Return to citationMarnitz, L., Rott, K., Niehörster, S., Klewe, C., Meier, D., Fabretti, S., Witziok, M., Krampf, A., Kuschel, O., Schemme, T., Kuepper, K., Wollschläger, J., Thomas, A., Reiss, G. & Kuschel, T. (2015). AIP Advances 5, 047103.  Google Scholar
Return to citationMishra, R. K. & Thomas, G. (1977). J. Appl. Phys. 48, 4576–4580.  CrossRef CAS Google Scholar
Return to citationMonti, M., Sanz, M., Oujja, M., Rebollar, E., Castillejo, M., Pedrosa, F. J., Bollero, A., Camarero, J., Cuñado, J. L. F., Nemes, N. M., Mompean, F. J., Garcia-Hernández, M., Nie, S., McCarty, K. F., N'Diaye, A. T., Chen, G., Schmid, A. K., Marco, J. F. & de la Figuera, J. (2013). J. Appl. Phys. 114, 223902.   Google Scholar
Return to citationMoussy, J.-B. (2013). J. Phys. D Appl. Phys. 46, 143001.  Web of Science CrossRef Google Scholar
Return to citationMoyer, J. A., Kumah, D. P., Vaz, C. A. F., Arena, D. A. & Henrich, V. E. (2012). Appl. Phys. Lett. 101, 021907.   Google Scholar
Return to citationPohlmann, T., Hoppe, M., Thien, J., Dey, A. B., Alexander, A., Ruwisch, K., Gutowski, O., Röh, J., Gloskovskii, A., Schlueter, C., Küpper, K., Wollschläger, J. & Bertram, F. (2022). Phys. Rev. B 105, 045412.  CrossRef Google Scholar
Return to citationRamos, R., Anadón, A., Lucas, I., Uchida, K., Algarabel, P. A., Morellón, L., Aguirre, M. H., Saitoh, E. & Ibarra, M. R. (2016). APL Mater. 4, 104802.  Google Scholar
Return to citationRamos, R., Kikkawa, T., Uchida, K., Adachi, H., Lucas, I., Aguirre, M. H., Algarabel, P., Morellón, L., Maekawa, S., Saitoh, E. & Ibarra, M. R. (2013). Appl. Phys. Lett. 102, 072413.   Google Scholar
Return to citationRodewald, J., Thien, J., Pohlmann, T., Hoppe, M., Timmer, F., Bertram, F., Kuepper, K. & Wollschläger, J. (2019). Phys. Rev. B 100, 155418.  CrossRef Google Scholar
Return to citationRodewald, J., Thien, J., Ruwisch, K., Bertram, F., Kuepper, K. & Wollschläger, J. (2020). Phys. Rev. Mater. 4, 064404.  CrossRef Google Scholar
Return to citationRubio-Zuazo, J., Onandia, L., Salas-Colera, E., Muñoz-Noval, A. & Castro, G. R. (2015). J. Phys. Chem. C 119, 1108–1112.  CAS Google Scholar
Return to citationSantos-Carballal, D., Roldan, A., Grau-Crespo, R. & de Leeuw, N. H. (2014). Phys. Chem. Chem. Phys. 16, 21082–21097.  CAS PubMed Google Scholar
Return to citationScherrer, P. (1918). Bestimmung der inneren Struktur und der Größe von Kolloidteilchen mittels Röntgenstrahlen, pp. 98–100. Berlin: Weidmannsche Buchhandlung.  Google Scholar
Return to citationSeneor, P., Fert, A., Maurice, J.-L., Montaigne, F., Petroff, F. & Vaurès, A. (1999). Appl. Phys. Lett. 74, 4017–4019.  CrossRef CAS Google Scholar
Return to citationTakahashi, R., Misumi, H. & Lippmaa, M. (2012). Cryst. Growth Des. 12, 2679–2683.  CrossRef CAS Google Scholar
Return to citationTakahashi, R., Misumi, H. & Lippmaa, M. (2014). J. Appl. Phys. 116, 033918.   Google Scholar
Return to citationThien, J., Bahlmann, J., Alexander, A., Hoppe, M., Pohlmann, T., Ruwisch, K., Meyer, C., Bertram, F., Küpper, K. & Wollschläger, J. (2020). J. Phys. Chem. C 124, 23895–23904.  CrossRef CAS Google Scholar
Return to citationTobin, J. G., Morton, S. A., Yu, S. W., Waddill, G. D., Schuller, I. K. & Chambers, S. A. (2007). J. Phys. Condens. Matter 19, 315218.  CrossRef PubMed Google Scholar
Return to citationUchida, K., Adachi, H., Kikkawa, T., Kirihara, A., Ishida, M., Yorozu, S., Maekawa, S. & Saitoh, E. (2016). Proc. IEEE 104, 1946–1973.  CrossRef CAS Google Scholar
Return to citationvan der Zaag, P. J., Bloemen, P. J. H., Gaines, J. M., Wolf, R. M., van der Heijden, P. A. A., van de Veerdonk, R. J. M. & de Jonge, W. J. M. (2000). J. Magn. Magn. Mater. 211, 301–308.   CrossRef CAS Google Scholar
Return to citationVassent, J. L., Dynna, M., Marty, A., Gilles, B. & Patrat, G. (1996). J. Appl. Phys. 80, 5727–5735.  CrossRef CAS Google Scholar
Return to citationWada, E., Watanabe, K., Shirahata, Y., Itoh, M., Yamaguchi, M. & Taniyama, T. (2010). Appl. Phys. Lett. 96, 102510.   Google Scholar
Return to citationWollschläger, J. (2018). Encyclopedia of Interfacial Chemistry, Vol. 3.1, pp. 284–296. Elsevier.  Google Scholar
Return to citationWollschläger, J., Erdös, D., Goldbach, H., Höpken, R. & Schröder, K. M. (2001). Thin Solid Films 400, 1–8.   Google Scholar
Return to citationYu, X., Huo, C.-F., Li, Y.-W., Wang, J. & Jiao, H. (2012). Surf. Sci. 606, 872–879.   CrossRef CAS Google Scholar
Return to citationZhang, Z. & Satpathy, S. (1991). Phys. Rev. B 44, 13319–13331.  CrossRef CAS Google Scholar

This is an open-access article distributed under the terms of the Creative Commons Attribution (CC-BY) Licence, which permits unrestricted use, distribution, and reproduction in any medium, provided the original authors and source are cited.

Journal logoJOURNAL OF
APPLIED
CRYSTALLOGRAPHY
ISSN: 1600-5767
Follow J. Appl. Cryst.
Sign up for e-alerts
Follow J. Appl. Cryst. on Twitter
Follow us on facebook
Sign up for RSS feeds